A LF refining method and device

By adjusting the power level and argon gas flow according to the slag conditions during the LF refining process, and optimizing the heating process, the problems of high power consumption and high cost in the existing technology are solved, and the effect of reducing power consumption and production costs is achieved.

CN116334353BActive Publication Date: 2024-10-18SGIS SONGSHAN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310538154.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-10-18
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

Due to poor submergence arc in the existing LF refining process, the heating efficiency is low, resulting in a large amount of power consumption and increased production costs. Improper operation will cause the temperature of the reinforced steel head to drop, increase the electricity bill and reduce the gross profit.

Method used

When there is slag or alloy lumps in the LF furnace, use low-level power transmission and high-argon stirring. After the slag addition is completed, switch to low-argon stirring. After judging that the refining situation meets the preset conditions, increase the level. power and reduce the argon gas flow to optimize the heating process.

Benefits of technology

By optimizing power usage and argon gas mixing flow, power consumption is reduced, production costs are reduced, and the efficiency of adding steel bars is improved to avoid temperature drop losses and increase gross profit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116334353B_ABST
    Figure CN116334353B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a LF refining method and device at a low iron-steel ratio, which relates to the field of metallurgical technology. The method includes: during the steelmaking process, determining whether there is slag or alloy agglomeration in the LF furnace. When there is slag or alloy agglomeration in the LF furnace, supplying power to the LF furnace based on the low gear, and supplying slag and steel bar heads into the LF furnace and stirring the slag with a first preset flow rate of argon. After the slag is added, supplying power and stirring the slag with a second preset flow rate of argon, determining the refining situation in the LF furnace, and judging whether the refining situation meets the preset conditions. When the situation in the LF furnace meets the preset conditions, supplying power to the LF furnace based on the high gear and stirring with a third preset flow rate of argon until the temperature in the LF furnace reaches the preset temperature. During the slagging period, a low gear is selected, and during the heating period, a high gear is selected to reduce power consumption and reduce costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metallurgical technology, and in particular to a LF refining method and device. Background Art

[0002] Due to the large fluctuations in scrap steel prices, production organization often changes. When scrap steel prices are cheap, more scrap steel and less molten iron are required. Therefore, in the prior art, in order to reduce the iron-steel ratio, that is, to use more scrap steel and less molten iron, it is required that ordinary carbon steel, screw steel and other steels with low quality requirements, use 3-5 tons of steel bar heads when the molten steel is refining LF. Based on 120 tons of molten steel, every 1.2 tons added can reduce the iron-steel ratio by 10 kg. For this reason, in order to spend as much refining time as possible on adding steel bar heads, the operator usually adds all the slag at one time after the molten steel reaches the processing position, and stirs with 100 cubic meters / hour of argon gas at the same time, uses high-grade gear, that is, 4-2 gear power transmission, active power 12500-15000KW, and adds steel bar heads while powering. The operator is used to quickly add the steel bar heads first, and then control the outlet temperature and molten steel composition until the continuous casting requirements are met when the LF is out of the station.

[0003] In the existing method, 2 or 4 gears are usually used for power transmission throughout the LF refining process, which reduces the iron-steel ratio and causes the LF refining process to consume a lot of electricity, especially in the early stage of refining (0-5 minutes after power transmission). Due to poor arcing, the heating efficiency is greatly reduced. For example, under normal circumstances, the temperature can be raised by 6°C per minute at 4 gear. However, during the early slag making, the arcing is not good and the temperature can only be raised by 3.5°C. With 4 gear power transmission, the reading per second is 3, the conversion efficiency is 0.6, the temperature rises by 1°C every 10 seconds, and the electricity price is 0.68 yuan / kWh. The cost of raising the temperature of molten steel by 1°C is 3×10÷0.6×0.68=34 yuan, which means that every minute is wasted. The power consumption is (6-3.5)*34=85 yuan, and the power consumption wasted in the first 5 minutes is 85*5=425 yuan, which results in a higher LF refining cost and the benefit brought by reducing the iron-steel ratio is not as high as expected. If the operation is improper, it will also lead to a greater temperature drop of the rebar head. That is, the budget is to add 1 ton of rebar head to reduce the temperature by 12℃, and the electricity bill will increase by 270 yuan. If the control is not good, 1 ton of rebar head can be cooled by 15℃, and the electricity bill will increase by 337.5, and the net profit will be reduced by 67.5 yuan. The speed of adding rebar head is 1 ton every 2 minutes. 2.5 tons can be added in the first 5 minutes of refining, and the initial waste cost is 2.5*67.5=168.75 yuan. In summary, under normal conditions, adding steel bar heads to reduce the temperature by 12℃ will increase the electricity cost by 270 yuan. If the above-mentioned wasted costs are added, the additional cost of adding steel bar heads in the early stage of refining is 168.75+425=593.75 yuan. If the gross profit of adding 1 ton of steel bar heads is 300 yuan, the original budget for adding 1 ton of steel bar heads is 30 yuan, but now 593.75 yuan is wasted, which is equivalent to adding 2 tons of steel bar heads in vain. Improper operation in the middle and late stages will also increase the electricity cost. Summary of the invention

[0004] The object of the present invention is to provide a LF refining method and device at a low iron-to-steel ratio, which can reduce the power consumption of LF refining and cut down the cost.

[0005] In order to achieve the above purpose, the technical solution adopted in the embodiment of the present application is as follows:

[0006] In a first aspect, an embodiment of the present application provides a LF refining method at a low iron-to-steel ratio, the method comprising:

[0007] During the steelmaking process, determine whether there is slag or alloy agglomeration in the LF furnace;

[0008] When the slag or the alloy agglomerate exists in the LF furnace, power is supplied to the LF furnace based on a low gear, and the slag and the steel bar head are fed into the LF furnace and the argon gas with a first preset flow rate is used to stir the slag;

[0009] After the slag material is added, power is supplied, and argon gas with a second preset flow rate is used to stir the slag material, wherein the first preset flow rate is greater than the second preset flow rate;

[0010] Determine the refining conditions in the LF furnace, and judge whether the refining conditions meet preset conditions, wherein the preset conditions include at least one of the following: detect that there is no arc light penetrating in the LF furnace or detect that there is no slag collision sound in the LF furnace;

[0011] When the situation in the LF furnace meets the preset conditions, the LF furnace is powered on based on a high gear and stirred with argon gas at a third preset flow rate until the temperature in the LF furnace reaches a preset temperature, wherein the third preset flow rate is less than the second preset flow rate.

[0012] In an optional embodiment, after the slag is added, the step of stirring the slag with argon gas at a second preset flow rate comprises:

[0013] After the slag is added, according to a preset cycle, the second preset flow rate is switched to the first preset flow rate and the slag is stirred according to the stirring time until the slag or alloy agglomerates in the LF furnace are melted.

[0014] In an optional embodiment, the method further comprises:

[0015] Determining fluidity in the LF furnace;

[0016] Based on the fluidity, it is determined whether fluorite or ferrosilicon powder needs to be added to the LF furnace.

[0017] In an optional embodiment, the step of determining the fluidity in the LF furnace comprises:

[0018] Providing argon gas at a fourth preset flow rate into the LF furnace to determine whether slag on the surface of the molten steel in the LF furnace or slag at the argon port flows;

[0019] The slag on the surface of the molten steel in the LF furnace and the slag at the argon port flow, and the fluidity in the LF furnace is determined to be the first fluidity;

[0020] If the slag on the surface of the molten steel in the LF furnace does not flow, and the slag at the argon port flows, the fluidity in the LF furnace is determined to be the second fluidity;

[0021] The step of determining whether fluorite or ferrosilicon powder needs to be added to the LF furnace based on fluidity includes:

[0022] When the fluidity is the first fluidity, it is determined that there is no need to add fluorite or ferrosilicon powder into the LF furnace;

[0023] When the fluidity is the second fluidity, it is determined that fluorite or ferrosilicon powder is added to the LF furnace.

[0024] In an optional embodiment, the method further comprises:

[0025] Determining the foaming condition in the LF furnace;

[0026] Based on the foaming condition, it is determined whether fluorite, ferrosilicon powder, aluminum particles and yellow mud need to be added to the LF furnace.

[0027] In an optional embodiment, the step of determining whether it is necessary to add fluorite, ferrosilicon powder, aluminum particles and yellow mud to the LF furnace based on the foamability condition comprises:

[0028] If the foaming condition of the slag in the LF furnace indicates that the amount of foaming is greater than a preset amount, it is determined that fluorite, ferrosilicon powder, aluminum particles and yellow mud are added to the LF furnace;

[0029] If the foaming condition of the slag in the LF furnace indicates that the foaming amount is less than the preset amount, it is determined that there is no need to add fluorite, ferrosilicon powder, aluminum particles and yellow mud into the LF furnace.

[0030] In an optional embodiment, the method further comprises:

[0031] Determine whether the steel bar head is rusty;

[0032] When the steel bar head is rusted, a third preset weight of slag is added into the LF furnace.

[0033] In an optional implementation, the first preset flow rate is 100 cubic meters per hour; the second preset flow rate is 50-60 cubic meters per hour; and the third preset flow rate is 20-50 cubic meters per hour.

[0034] In an optional embodiment, the low gear includes gears 8-11, and the high gear includes gears 2-4.

[0035] In a second aspect, an embodiment of the present application provides a LF refining device at a low iron-to-steel ratio, the device further comprising:

[0036] The first determination module is used to determine whether there is slag or alloy agglomeration in the LF furnace during the steelmaking process;

[0037] a first control module, configured to supply power to the LF furnace based on a low gear when the slag or the alloy agglomerate exists in the LF furnace, and to supply the slag and the steel bar head into the LF furnace and stir the slag with argon gas of a first preset flow rate;

[0038] A second control module is used to supply power after the slag material is added, and stir the slag material with argon gas at a second preset flow rate, wherein the first preset flow rate is greater than the second preset flow rate;

[0039] The second determination module is used to determine the refining situation in the LF furnace and judge whether the refining situation meets the preset conditions, wherein the preset conditions include at least one of the following: detecting that there is no arc light penetrating in the LF furnace and detecting that there is no slag collision sound in the LF furnace;

[0040] The third control module is used to supply power to the LF furnace based on a high gear and stir it with argon gas at a third preset flow rate when the situation in the LF furnace meets the preset conditions until the temperature in the LF furnace reaches the preset temperature, wherein the third preset flow rate is less than the second preset flow rate.

[0041] In a third aspect, an embodiment of the present application provides a LF refining device, including a memory and a processor, wherein the memory stores a computer program, and the processor implements the steps of the LF refining method at a low iron-to-steel ratio when executing the computer program.

[0042] In a fourth aspect, an embodiment of the present application provides a computer-readable storage medium having a computer program stored thereon, which, when executed by a processor, implements the steps of the LF refining method at a low iron-steel ratio.

[0043] This application has the following beneficial effects:

[0044] The present application determines whether there is slag or alloy agglomeration in the LF furnace during the steelmaking process. When there is slag or alloy agglomeration in the LF furnace, the LF furnace is powered on based on the low gear, and the slag and the steel bar head are fed into the LF furnace and the slag is stirred with the first preset flow rate of argon. After the slag is added, power is supplied and the slag is stirred with the second preset flow rate of argon, wherein the first preset flow rate is greater than the second preset flow rate, the refining situation in the LF furnace is determined, and whether the refining situation meets the preset conditions, wherein the preset conditions include at least one of the following: detecting that there is no arc light penetrating in the LF furnace or detecting that there is no slag block collision sound in the LF furnace. When the situation in the LF furnace meets the preset conditions, the LF furnace is powered on based on the high gear and stirred with the third preset flow rate of argon until the temperature in the LF furnace reaches the preset temperature, wherein the third preset flow rate is less than the second preset flow rate. During the slagging period, the low gear is selected, and during the heating period, the high gear is selected to reduce power consumption and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0046] Figure 1 A block diagram of a LF refining device provided by an embodiment of the present invention;

[0047] Figure 2 One of the flow diagrams of a LF refining method at a low iron-to-steel ratio provided by an embodiment of the present invention;

[0048] Figure 3 A second flow chart of a LF refining method at a low iron-to-steel ratio provided by an embodiment of the present invention;

[0049] Figure 4 A third flow chart of a LF refining method at a low iron-to-steel ratio provided by an embodiment of the present invention;

[0050] Figure 5 A fourth flow chart of a LF refining method at a low iron-to-steel ratio provided by an embodiment of the present invention;

[0051] Figure 6 A structural block diagram of a LF refining device at a low iron-to-steel ratio provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0053] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0055] In the description of the present invention, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, they are based on the orientation or position relationship shown in the accompanying drawings, or are the orientation or position relationship in which the product of the invention is usually placed when used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0056] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.

[0057] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0058] After extensive research by the inventors, it was found that in the prior art, 2 or 4 gears are usually used for power transmission throughout the LF refining process, which reduces the iron-steel ratio while causing the LF refining process to consume a large amount of electricity, especially in the early stage of refining (0-5 minutes after power transmission). Due to poor arcing, the heating efficiency is greatly reduced. For example, under normal circumstances, the temperature can be raised by 6°C per minute at 4 gear. However, during the early slag making, the arcing is not good and the temperature can only be raised by 3.5°C. With 4 gear power transmission, the reading per second is 3, the conversion efficiency is 0.6, the temperature rises by 1°C every 10 seconds, and the electricity price is 0.68 yuan / kWh. The cost of raising the temperature of the molten steel by 1°C is 3×10÷0.6×0.68=34 yuan. The electricity wasted per minute is (6-3.5)*34=85 yuan, and the electricity wasted in the first 5 minutes is 85*5=425 yuan, which results in a higher LF refining cost and the benefit brought by reducing the iron-steel ratio is not as high as expected. If the operation is improper, it will also lead to a greater drop in the temperature of the rebar heads. That is, the budget is to add 1 ton of rebar heads to reduce the temperature by 12°C, and the electricity bill will increase by 270 yuan. If it is not well controlled, 1 ton of rebar heads can be cooled by 15°C, and the electricity bill will increase by 337.5, and the net profit will be reduced by 67.5 yuan. The speed of adding rebar heads is 1 ton every 2 minutes. 2.5 tons can be added in the first 5 minutes of refining, and the initial waste cost is 2.5*67.5=168.75 yuan. In summary, under normal conditions, adding steel bar heads to reduce the temperature by 12℃ will increase the electricity cost by 270 yuan. If the above-mentioned wasted costs are added, the additional cost of adding steel bar heads in the early stage of refining is 168.75+425=593.75 yuan. If the gross profit of adding 1 ton of steel bar heads is 300 yuan, the original budget for adding 1 ton of steel bar heads is 30 yuan, but now 593.75 yuan is wasted, which is equivalent to adding 2 tons of steel bar heads in vain. Improper operation in the middle and late stages will also increase the electricity cost.

[0059] In view of the discovery of the above problems, the present embodiment provides a LF refining method and device at a low iron-steel ratio, which can select a low gear during slag reduction and a high gear during heating, thereby reducing power consumption and reducing costs. The solution provided in this embodiment is described in detail below.

[0060] This embodiment provides an LF refining device capable of controlling LF refining.

[0061] Please refer to Figure 1 , Figure 1 1 is a schematic diagram of the structure of the LF refining equipment 100 provided in the embodiment of the present application. The LF refining equipment 100 may also include Figure 1 More or fewer components as shown, or with Figure 1 Different configurations are shown. Figure 1 Each component shown in the figure can be implemented by hardware, software or a combination thereof.

[0062] The LF refining equipment 100 includes a low iron-steel ratio LF refining device 110 , a memory 120 and a processor 130 .

[0063] The memory 120 and the processor 130 are electrically connected to each other directly or indirectly to achieve data transmission or interaction. For example, these elements can be electrically connected to each other through one or more communication buses or signal lines. The LF refining device 110 at low iron-steel ratio includes at least one software function module that can be stored in the memory 120 in the form of software or firmware or solidified in the operating system (OS) of the LF refining device 100 at low iron-steel ratio. The processor 130 is used to execute the executable modules stored in the memory 120, such as the software function modules and computer programs included in the LF refining device 110.

[0064] The memory 120 may be, but is not limited to, a random access memory (RAM), a read only memory (ROM), a programmable read-only memory (PROM), an erasable programmable read-only memory (EPROM), an electrically erasable read-only memory (EEPROM), etc. The memory 120 is used to store a program, and the processor 130 executes the program after receiving an execution instruction.

[0065] Please refer to Figure 2 , Figure 2 For application Figure 1 A flow chart of a LF refining method at a low iron-to-steel ratio of the LF refining equipment 100 is shown, and the method including various steps is described in detail below.

[0066] Step 201: During the steelmaking process, determine whether there is slag or alloy agglomerates in the LF furnace.

[0067] Step 202: When there is slag or the alloy agglomerates in the LF furnace, power is supplied to the LF furnace at a low gear, and slag and steel bar heads are fed into the LF furnace and stirred with argon gas at a first preset flow rate.

[0068] Step 203: After the slag material is added, power is supplied and the slag material is stirred with argon gas at a second preset flow rate.

[0069] Among them, the first preset flow rate is greater than the second preset flow rate.

[0070] Step 204: Determine the refining conditions in the LF furnace and judge whether the refining conditions meet the preset conditions.

[0071] The preset condition includes at least one of the following: detecting that there is no arc light penetrating from the LF furnace and detecting that there is no slag collision sound in the LF furnace.

[0072] Step 205: When the situation in the LF furnace meets the preset conditions, power is supplied to the converter based on the high-speed position, and argon gas with a third preset flow rate is used for stirring until the temperature in the LF furnace reaches the preset temperature.

[0073] The third preset flow rate is smaller than the second preset flow rate.

[0074] Exemplarily, during steelmaking, the station determines the slag washing condition in the LF furnace, including whether slag or alloy agglomerates are contained, and supplies power to the LF furnace based on the slag washing condition of the LF furnace. If there is no slag or alloy agglomerates in the LF furnace, power is supplied to the LF furnace based on the low gear. If there is slag or alloy agglomerates in the LF furnace, power is supplied to the LF based on the low gear, and slag and steel bar heads are fed into the LF furnace, and in order to melt the slag, argon gas of a first preset flow rate is used for stirring.

[0075] The purpose of feeding slag into the LF furnace is that if slag is not fed into the LF furnace, the unmelted slag in the ladle will clump together, resulting in a thin slag layer in the ladle, or less slag, resulting in poor submerged arc effect, thereby causing a large amount of power consumption. Feeding slag into the LF furnace can improve the submerged arc effect, thereby reducing power consumption.

[0076] Exemplarily, slag having a total weight of a first preset weight may be fed into the LF furnace.

[0077] It should be noted that slag is added to the LF furnace multiple times, and the total weight of the added slag is the first preset weight, wherein the first preset weight can be set to 300-500 kg, and the first preset flow rate can be set to 100-120 cubic meters / hour. Those skilled in the art can feed slag into the LF furnace according to the actual situation of steelmaking, and the present application does not limit the total weight of the fed slag to 300-500 kg.

[0078] It should be noted that, when the first preset flow rate is set, if a small flow rate of argon is used for slag melting, the particles of the slag produced will be larger or coarser, the gaps between the slags will be larger, and arc light will pass through the gaps, resulting in a waste of electricity.

[0079] There are multiple options for the low gear. In one example, the low gear can be set to gears 8-11.

[0080] Among them, the 8th gear collects a value of 2 per second, the temperature rises by 4 degrees Celsius per minute, and the conversion efficiency is 0.58. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 8th gear is 10 / 4*60*2 / 0.58=517. The 9th gear collects a value of 1.7 per second, the temperature rises by 3.5 degrees Celsius per minute, and the conversion efficiency is 0.62. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 9th gear is 10 / 3.5*60*1.7 / 0.62=470. The 10th gear collects a value of 1.3 per second, the temperature rises by 2.7 degrees Celsius per minute, and the conversion efficiency is 0.59. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 10th gear is 10 / 2.7*60*1.3 / 0.59=490. The 11th gear collects a value of 1 per second, the temperature rises by 2 degrees Celsius per minute, and the conversion efficiency is 0.61. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 8th gear is 10 / 2*60*1 / 0.61=492.

[0081] Exemplarily, when there is slag or the alloy agglomerates in the LF furnace, power is supplied to the LF furnace based on the 9th gear, and the heating effect based on the 9th gear is the best and the power consumption is the lowest.

[0082] Exemplarily, a second preset weight of steel bar heads is added to the LF furnace, and the sum of the second preset weight and the weight of the slag and alloy agglomerates currently in the LF furnace is less than the maximum weight that can be added to the LF furnace.

[0083] There are many ways to add steel bar heads to the LF furnace. In one implementation, during the power supply process to the LF furnace, the clearance of the LF furnace is determined in real time, and based on the clearance of the LF furnace, a second preset weight of steel bar heads is added to the LF furnace. Exemplarily, when the clearance of the LF furnace is 7 tons, based on the steelmaking process cycle, the second preset weight of steel bar heads added to the LF furnace each time is determined, for example, the second preset weight is 1 ton, 2 tons, 3 tons, etc.

[0084] In another implementation, the clearance distance in the LF furnace is determined, and when the clearance distance in the LF furnace is less than a preset distance, slag is added into the LF furnace.

[0085] It should be noted that the first preset distance can be set to 40CM.

[0086] Generally speaking, when the clearance in the LF furnace, that is, the distance from the furnace mouth to the molten steel surface, is greater than 40CM, there is no need to add lime. However, with the addition of steel bar heads, the molten steel surface will become fuller and fuller. When the clearance distance in the LF furnace is less than 40CM, more and more slag will be splashed out by the reaction force of the electrode during the power transmission process, resulting in a thinner slag layer and a poor submerged arc effect. Therefore, 130-190 kg of slag is added to the LF furnace to supplement the slag layer thickness, thereby meeting the submerged arc effect and reducing power consumption.

[0087] Here, the slag filling needs to be carried out according to the remaining power supply time. Usually, the slag filling is required only when the remaining power supply time is calculated to be greater than 2.5 minutes (calculated at 4-speed heating, the molten steel temperature still needs to be raised by more than 15°C). Calculated as adding 190 kg of lime, the cost is 0.66 yuan per kg, and the cost is 190*0.66=125.4 yuan. The power is transmitted at 4th gear, the reading per second is 3, the conversion efficiency is 0.6, the temperature rises by 1°C every 10 seconds, the electricity price is 0.68 yuan / kWh, and the cost of 1°C higher temperature of molten steel is 3×10÷0.6×0.68=34 yuan. The temperature rises by 6°C per minute when the arc is good and 4.5°C per minute when the arc is poor. On the basis of the remaining power transmission time of 2.5 minutes, the temperature rises by 2.5-(6-4.5)=3.75°C less, and the electricity consumption cost is 3.75*34=127.5 yuan. Therefore, when the operator finds that the arc effect is poor and the remaining heating time is less than 2.5 minutes, there is no need to add slag.

[0088] Through practice, it is found that the submerged arc will deteriorate after adding 3 tons or more of steel bar heads. When the ladle clearance is 50-70 cm, it can be estimated that the molten steel level will be less than 50 cm after adding the steel bar heads. In this case, about 150 kg of lime will be added in the early or middle stage to avoid the deterioration of the submerged arc and increase in power consumption in the later stage.

[0089] When adding slag and steel bar heads into the LF furnace, the added slag and steel bar heads cannot exceed the maximum clearance of the LF furnace.

[0090] When power is supplied to the LF furnace based on the low gear, the material and the steel bar head are fed into the LF furnace and the slag is stirred with argon at a first preset flow rate. After the slag is added, the slag is stirred with argon at a second preset flow rate, and the refining situation in the LF furnace is determined in real time. Whether the slag is completely melted is judged according to the refining situation. The determination method can be: determining whether the refining situation in the LF furnace meets the preset conditions, the refining situation in the LF furnace indicates that there is no arc light transmitted in the LF furnace, or the refining situation in the LF furnace indicates that there is no slag block collision sound in the LF furnace. When the refining situation meets the above preset conditions, it is determined that the slag is completely melted. When the slag is completely melted, power is supplied to the LF furnace based on the high gear, and argon at a third preset flow rate is used for stirring, so that the molten steel in the LF furnace can be quickly heated up.

[0091] Exemplarily, there may be a variety of options for the high gear. In one example, the high gear may be set to gears 2-4.

[0092] Among them, the value collected per second in the 2nd gear is 4, the temperature rises by 8 degrees Celsius per minute, and the conversion efficiency is 0.58. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 2nd gear is 10 / 8*60*4 / 0.58=517. The value collected per second in the 3rd gear is 3.5, the temperature rises by 7 degrees Celsius per minute, and the conversion efficiency is 0.59. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 3rd gear is 10 / 7*60*3.5 / 0.59=508. The value collected per second in the 4th gear is 3, the temperature rises by 6 degrees Celsius per minute, and the conversion efficiency is 0.6. Taking the temperature rise of 120 tons of molten steel by 10 degrees Celsius as an example, the power consumption of the 4th gear is 10 / 6*60*3 / 0.6=500.

[0093] Exemplarily, when the refining conditions in the LF furnace meet the preset conditions, the slag is stirred with argon gas at a third preset flow rate, and the heating effect based on the 4th gear is the best and the power consumption is the lowest.

[0094] It should be noted that the second preset flow rate can be set to 50-60 square meters / hour, and the embodiment of the present application does not impose any specific restrictions on the second preset flow rate. Those skilled in the art can set the second preset flow rate according to actual conditions.

[0095] The third preset flow rate can be set to 20-50 cubic meters per hour. Those skilled in the art can adjust the third preset flow rate according to actual conditions. The present application does not make any specific limitation on the third preset flow rate.

[0096] It should be noted that when the refining conditions meet the preset conditions, it is determined that the slag is completely melted. At this time, the temperature in the LF furnace needs to be heated to the preset temperature. If the argon control is too large, the molten steel will roll too much, resulting in poor arc submergence effect, and the arc will penetrate from the slag. If the argon control is too small, it will also cause the top molten steel to transfer heat slowly or less downward, resulting in the heat of the top molten steel being extracted by dust removal, resulting in a slow heating speed in the LF furnace. The optimal value of the argon flow rate is the maximum flow rate when the arc submergence effect is good. Therefore, with the appropriate third preset flow rate of argon stirring, the power consumption can be reduced under the condition of better heating effect. For example, 25 cubic meters / hour of argon and 35 cubic meters / hour of argon can both bury the arc well, and the heating will be faster with 35 cubic meters / hour of argon.

[0097] After the slag is added, the slag is stirred at a second preset flow rate so that the slag or alloy agglomerates in the LF furnace are completely melted. There are multiple implementation methods. In one implementation method, the method includes:

[0098] After the slag is added, according to the preset cycle, the second preset flow rate is switched to the first preset flow rate and the slag is stirred according to the stirring time until the slag or alloy agglomerates in the LF furnace are melted.

[0099] Exemplarily, after the slag is added, the slag is stirred by switching the second preset flow rate of 50-60 cubic meters / hour to the first preset flow rate of 100-120 cubic meters / hour of argon every two minutes, and the stirring time based on 100-120 cubic meters / hour of argon is 5-60 seconds.

[0100] According to the preset cycle, the second preset flow rate is switched to the first preset flow rate, and the slag is stirred according to the stirring time, which can promote the melting of the slag and reduce power consumption. If the argon flow rate switched according to the preset cycle is small during the slag melting stage, the slag particles will be larger or coarser, the gaps between the slags will be larger, and the arc will pass through the gaps, resulting in a waste of power consumption.

[0101] There are many ways to reduce power consumption during the refining process. In one implementation, Figure 3 As shown, the following steps are included:

[0102] Step 301: Determine the fluidity in the LF furnace.

[0103] Step 303: Based on the fluidity, determine whether fluorite or ferrosilicon powder needs to be added to the LF furnace.

[0104] There are many ways to determine the fluidity in the LF furnace. In one implementation, the following steps are included: adding argon gas at a fourth preset flow rate to the LF furnace to determine whether the slag on the surface of the molten steel in the LF furnace or the slag at the argon port flows. If the slag on the surface of the molten steel in the LF furnace and the slag at the argon port flow, the fluidity in the LF furnace is determined to be the first fluidity. If the slag on the surface of the molten steel in the LF furnace does not flow, and the slag at the argon port flows, the fluidity in the LF furnace is determined to be the second fluidity. When the fluidity is the first fluidity, it is determined that there is no need to add fluorite or ferrosilicon powder to the LF furnace; when the fluidity is the second fluidity, it is determined that fluorite or ferrosilicon powder is added to the LF furnace.

[0105] The fluidity of the slag must be controlled during the power transmission process. The slag fluidity must be good, that is, the argon gas is controlled during weak blowing, that is, weak blowing is performed according to the fourth preset flow rate of 10-20 cubic meters / hour of argon gas. The slag on the entire surface of the molten steel fluctuates. If only the slag at the argon port flows on the liquid surface, and the slag in other places does not move, it indicates that the fluidity in the LF furnace is the second fluidity, indicating that the fluidity is not enough. Fluorite or ferrosilicon powder needs to be added until the fluidity is good. When the slag fluidity is the second fluidity, it will directly affect the heat transfer speed and the submerged arc effect, resulting in high power consumption.

[0106] There are many ways to reduce power consumption during the refining process. In one implementation, Figure 4 As shown, the following steps are included:

[0107] Step 401: Determine the foaming condition in the LF furnace.

[0108] Step 402: Based on the foaming condition, determine whether it is necessary to add fluorite, ferrosilicon powder, aluminum particles and yellow mud into the LF furnace.

[0109] Exemplarily, if the foaming condition of the slag in the LF furnace indicates that the amount of foaming is greater than a preset amount, it is determined that fluorite, ferrosilicon powder, aluminum particles and yellow mud are added to the LF furnace. If the foaming condition of the slag in the LF furnace indicates that the amount of foaming is less than a preset amount, it is determined that there is no need to add fluorite, ferrosilicon powder, aluminum particles and yellow mud to the LF furnace.

[0110] In another example, the foaming condition of the slag in the LF furnace may be determined manually.

[0111] When the foaming quantity indicated by the foaming condition of the slag in the LF furnace is greater than the preset quantity, it indicates that the foaming is too strong. When the foaming is strong, the thickness of the slag will be greatly increased, resulting in the electrode position rising, the depth of insertion into the molten steel becoming shallower, and the heating rate being greatly reduced. If the foaming condition of the slag in the LF furnace is too strong, then fluorite, ferrosilicon powder, aluminum particles and yellow mud will be added to the LF furnace. For example, if the LF furnace is powered on at level 4, one minute later, when the foaming condition in the LF furnace is complete, the temperature of the molten steel will rise by 6 degrees Celsius. If the foaming is strong and the foaming of the slag is not handled, the temperature of the molten steel will only rise by 4.5-5 degrees Celsius in one minute. Therefore, in order to reduce power consumption, when it is found that the slag foaming is more serious, fluorite, ferrosilicon powder, aluminum particles, yellow mud, etc. will be added to the LF furnace to eliminate the bubbles, thereby reducing power consumption.

[0112] There are many ways to reduce power consumption during the refining process. In one implementation, Figure 5 As shown, the following steps are included:

[0113] Step 501: Determine whether the steel bar head is rusted.

[0114] Step 502: When the steel bar head is rusted, a second preset mass of lime is added into the LF furnace.

[0115] Since different batches of rebar heads may be added to the LF furnace multiple times, the rust conditions of different batches of rebar heads are different. When the rust condition of the rebar heads is serious, the slag will be thinned, especially after adding 3 tons, which will make the original white gypsum slag turn into black glass slag. After the slag becomes thinner, the submerged arc effect becomes worse. Therefore, when it is determined that the rebar heads are rusted, add the third preset weight of slag to the LF furnace. The third preset weight can be set to 80-150 kg.

[0116] During LF refining, there may be other factors that increase the power consumption of LF refining, exemplified by:

[0117] Since the lifting and lowering control of the electrodes of the LF refining equipment is automatically controlled by collecting current and voltage values, as the equipment wears, the inspection accuracy or response ability decreases, resulting in the three-phase electrodes being out of sync. This phenomenon is manifested on the computer level 1 machine, resulting in a large difference between the three current curves. At this time, it is necessary to adjust the equipment parameters of the LF refining equipment, or to inspect the hydraulic control valves of the LF refining equipment.

[0118] If some steel grades do not allow the addition of steel bar heads, calculate the refining cycle in advance to ensure that power is supplied throughout the LF refining process and reduce the waiting time when power is not supplied.

[0119] Please refer to Figure 6 The present application embodiment also provides an application Figure 1 The LF refining device 110 with a low iron-steel ratio of the LF refining equipment 100 includes:

[0120] The first determination module 111 is used to determine whether there is slag or alloy agglomeration in the LF furnace during the steelmaking process;

[0121] The first control module 112 is used for supplying power to the LF furnace based on a low gear when the slag or the alloy agglomerate exists in the LF furnace, and supplying the slag and the steel bar head into the LF furnace and stirring the slag with argon gas of a first preset flow rate;

[0122] The second control module 113 is used to supply power after the slag material is added, and stir the slag material with argon gas at a second preset flow rate, wherein the first preset flow rate is greater than the second preset flow rate;

[0123] The second determination module 114 is used to determine the refining situation in the LF furnace and judge whether the refining situation meets the preset conditions, wherein the preset conditions include at least one of the following: detecting that there is no arc light penetrating in the LF furnace and detecting that there is no slag collision sound in the LF furnace;

[0124] The third control module 115 is used to supply power to the LF furnace based on a high gear when the situation in the LF furnace meets the preset conditions, and stir it with argon gas at a third preset flow rate until the temperature in the LF furnace reaches the preset temperature, wherein the third preset flow rate is less than the second preset flow rate.

[0125] The present application also provides a LF refining device 100, which includes a processor 130 and a memory 120. The memory 120 stores computer executable instructions, and when the computer executable instructions are executed by the processor 130, the LF refining method at low iron-steel ratio is implemented.

[0126] The embodiment of the present application also provides a computer-readable storage medium, which stores a computer program. When the computer program is executed by the processor 130, the LF refining method at low iron-steel ratio is implemented.

[0127] In the embodiments provided in the present application, it should be understood that the disclosed devices and methods can also be implemented in other ways. The device embodiments described above are merely schematic. For example, the flowcharts and block diagrams in the accompanying drawings show the possible architecture, functions and operations of the devices, methods and computer program products according to the multiple embodiments of the present application. In this regard, each box in the flowchart or block diagram can represent a module, a program segment or a part of a code, and the module, a program segment or a part of a code contains one or more executable instructions for implementing the specified logical function. It should also be noted that in some alternative implementations, the functions marked in the box can also occur in a different order from the order marked in the accompanying drawings. For example, two consecutive boxes can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, depending on the functions involved. It should also be noted that each box in the block diagram and / or the flowchart, and the combination of boxes in the block diagram and / or the flowchart can be implemented with a dedicated hardware-based system that performs a specified function or action, or can be implemented with a combination of dedicated hardware and computer instructions.

[0128] In addition, each functional module in each embodiment of the present application can be integrated together to form an independent part, or each module can exist separately, or two or more modules can be integrated to form an independent part. If the function is implemented in the form of a software functional module and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on such an understanding, the technical solution of the present application is essentially or the part that contributes to the prior art or the part of the technical solution can be embodied in the form of a software product, and the computer software product is stored in a storage medium, including several instructions to enable a computer device (which can be a personal computer, a server, or a network device, etc.) to perform all or part of the steps of the method described in each embodiment of the present application. The aforementioned storage medium includes: various media that can store program codes, such as a USB flash drive, a mobile hard disk, a read-only memory (ROM, Read-Only Memory), a random access memory (RAM, Random Access Memory), a disk or an optical disk.

[0129] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0130] The above are only various implementations of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A LF refining method with low iron-steel ratio, It is characterized in that The method comprises: During the steelmaking process, determine whether there is slag or alloy agglomeration in the LF furnace; When the slag or the alloy agglomerates exist in the LF furnace, power is supplied to the LF furnace at a low gear, and the slag and the steel bar heads are fed into the LF furnace and the argon gas with a first preset flow rate is used to stir the slag; After the slag material is added, power is supplied, and argon gas with a second preset flow rate is used to stir the slag material, wherein the first preset flow rate is greater than the second preset flow rate; Determine the refining conditions in the LF furnace, and judge whether the refining conditions meet preset conditions, wherein the preset conditions include at least one of the following: detect that there is no arc light penetrating in the LF furnace or detect that there is no slag collision sound in the LF furnace; When the situation in the LF furnace meets the preset conditions, the LF furnace is powered on based on a high gear and stirred with argon gas at a third preset flow rate until the temperature in the LF furnace reaches a preset temperature, wherein the third preset flow rate is less than the second preset flow rate.

2. The method according to claim 1, It is characterized in that The step of supplying power after the slag material is added and stirring the slag material with argon gas of a second preset flow rate comprises: After the slag is added, according to a preset cycle, the second preset flow rate is switched to the first preset flow rate and the slag is stirred according to the stirring time until the slag or alloy agglomerates in the LF furnace are melted.

3. The method according to claim 1, It is characterized in that The method further comprises: Determining fluidity in the LF furnace; Based on the fluidity, it is determined whether fluorite or ferrosilicon powder needs to be added to the LF furnace.

4. The method according to claim 3, It is characterized in that The step of determining the fluidity in the LF furnace comprises: Providing argon gas at a fourth preset flow rate into the LF furnace to determine whether slag on the surface of the molten steel in the LF furnace or slag at the argon port flows; The slag on the surface of the molten steel in the LF furnace and the slag at the argon port flow, and the fluidity in the LF furnace is determined to be the first fluidity; If the slag on the surface of the molten steel in the LF furnace does not flow, and the slag at the argon port flows, the fluidity in the LF furnace is determined to be the second fluidity; The step of determining whether fluorite or ferrosilicon powder needs to be added to the LF furnace based on the fluidity includes: When the fluidity is the first fluidity, it is determined that there is no need to add fluorite or ferrosilicon powder into the LF furnace; When the fluidity is the second fluidity, it is determined that fluorite or ferrosilicon powder is added to the LF furnace.

5. The method according to claim 1, It is characterized in that The method further comprises: Determining the foaming condition in the LF furnace; Based on the foaming condition, it is determined whether fluorite, ferrosilicon powder, aluminum particles and yellow mud need to be added to the LF furnace.

6. The method according to claim 5, It is characterized in that The step of determining whether it is necessary to add fluorite, ferrosilicon powder, aluminum particles and yellow mud into the LF furnace based on the foamability includes: If the foaming condition of the slag in the LF furnace indicates that the amount of foaming is greater than a preset amount, it is determined that fluorite, ferrosilicon powder, aluminum particles and yellow mud are added to the LF furnace; If the foaming condition of the slag in the LF furnace indicates that the foaming amount is less than the preset amount, it is determined that there is no need to add fluorite, ferrosilicon powder, aluminum particles and yellow mud into the LF furnace.

7. The method according to claim 1, It is characterized in that The method further comprises: Determine whether the steel bar head is rusty; When the steel bar head is rusted, a third preset weight of slag is added into the LF furnace.

8. The method according to claim 1, It is characterized in that The first preset flow rate is 100 cubic meters per hour; The second preset flow rate is 50-60 cubic meters per hour; The third preset flow rate is 20-50 cubic meters per hour.

9. The method according to claim 1, It is characterized in that The low gear includes gears 8-11, and the high gear includes gears 2-4.

10. A LF refining device with low iron-steel ratio, It is characterized in that The device also includes: The first determination module is used to determine whether there is slag or alloy agglomeration in the LF furnace during the steelmaking process; a first control module, configured to supply power to the LF furnace based on a low gear when the slag or the alloy agglomerate exists in the LF furnace, and to supply the slag and the steel bar head into the LF furnace and stir the slag with argon gas of a first preset flow rate; A second control module is used to supply power after the slag material is added, and stir the slag material with argon gas at a second preset flow rate, wherein the first preset flow rate is greater than the second preset flow rate; The second determination module is used to determine the refining situation in the LF furnace and judge whether the refining situation meets the preset conditions, wherein the preset conditions include at least one of the following: detecting that there is no arc light penetrating in the LF furnace and detecting that there is no slag collision sound in the LF furnace; The third control module is used to supply power to the LF furnace based on a high gear and stir it with argon gas at a third preset flow rate when the situation in the LF furnace meets the preset conditions until the temperature in the LF furnace reaches the preset temperature, wherein the third preset flow rate is less than the second preset flow rate.

Citation Information

Patent Citations

  • LF refining method under low iron-steel ratio

    CN115287397A

  • Method for quickly desulfurizing low-sulfur steel at low temperature under low iron-steel ratio

    CN116004947A