Method for synthesizing large-size diamond crystals using chemical vapor deposition
By using a three-layer substrate structure of single-crystal silicon, SiO2 film and TiCN film in the diamond synthesis process, and by etching and annealing, the problem of brittle fracture of large-size diamonds was solved, and high-quality diamond materials were prepared.
Patent Information
- Application Number
- CN202310355224.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-04-06
AI Technical Summary
Existing technologies suffer from brittle fracture and structural defects when synthesizing large-sized diamonds, making it difficult to achieve high-quality diamond material preparation.
A substrate is formed by a tight composite of three layers: single-crystal silicon, SiO2 film, and TiCN film. Through etching and annealing, the deposition environment and heat treatment method of diamond are optimized to enhance the bonding force between epitaxial growth and the substrate and reduce internal stress and structural defects.
This method enables stable growth of large-sized diamonds, avoids brittle fracture, and improves the mechanical properties and overall toughness of diamonds.
Smart Images

Figure CN116334752B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of diamond technology, specifically relating to a method for synthesizing large-size diamond crystals using chemical vapor deposition. Background Technology
[0002] Diamond, an allotrope of carbon (C), is a typical atomic crystal, in which each carbon atom forms four sp atoms. 3 The hybridized atomic orbitals form σ-type covalent single bonds with the four adjacent carbon atoms, resulting in a tetrahedral structure. This arrangement of carbon atoms and the characteristics of its crystal structure give diamond excellent physical properties: a large band gap (5.5 eV) and high carrier mobility (holes: 3800 cm⁻¹). 2 ·V -1 ·s -1 Electron: 4500cm 2 ·V -1 ·s -1 High breakdown field strength (>10MV·cm) -1 High thermal conductivity (22 W·K) -1 ·cm -1 Natural diamonds are characterized by their resistance to corrosion and biocompatibility. However, natural diamonds are scarce, have uneven purity, and are small in size, necessitating the development of synthetic diamond technology to obtain large-size, high-quality diamond materials.
[0003] Currently, the main methods for artificially synthesizing diamond are high-temperature high-pressure (HTHP) and chemical vapor deposition (CVD). HTHP involves causing a phase transition in graphite powder under high temperature and pressure to synthesize diamond; however, HTHP diamond synthesis typically requires high temperature and pressure, and the use of a metal catalyst during the synthesis process inevitably introduces impurities, affecting product quality. Compared to HTHP, CVD grows diamond in a low-pressure gas phase, reducing temperature requirements and providing the possibility of growing thin films on large-area substrates. The growth quality of diamond is highly correlated with substrate characteristics (temperature and crystal orientation, etc.) and process parameters (CH4 / H2 ratio, gas flow rate, and type of dopant gas, etc.). Research on large-size diamonds mainly focuses on substrate selection and process parameter control.
[0004] Patent CN110079860B discloses a method for splicing and growing large-size single-crystal diamond epitaxial wafers. First, multiple single-crystal diamond epitaxial wafers with strictly consistent crystal orientations are obtained through ion implantation and separation technology followed by chemical vapor deposition. Then, the epitaxial wafers are horizontally arranged along the consistent crystal orientation and bonded to a substrate. Planarization and ion implantation are then performed, and finally, large-size single-crystal diamond epitaxial wafers are obtained through chemical vapor deposition and separation. This method uses substrates with identical properties to prepare large-size diamond crystal materials; however, inappropriate mismatch can lead to cracking risks between substrates. Patent CN110230091B discloses a method for vertically splicing and preparing large-size CVD diamond and its cutting. Large-size CVD diamonds are epitaxially grown on the sides of multiple vertically and closely arranged single-crystal diamond seed crystals, and then the seed crystals and epitaxial diamonds are separated sequentially using laser cutting. However, as the number of seed crystals increases, the epitaxial growth rate and impurity concentration distribution become uneven, affecting the growth quality of the diamond. Furthermore, in the first two methods, the separation of the diamond epitaxial layer from the substrate causes damage to the diamond substrate. Patent CN111206280B discloses a method for high-quality, large-size single-crystal diamond epitaxial growth. This method involves precision polishing a large-size single-crystal diamond wafer grown using a mosaic-like splicing technique, followed by sequential deposition of metallic nickel and metallic iridium using electron beam evaporation. An amorphous carbon layer is then pre-deposited to promote carbon atom enrichment on the subsurface of the iridium thin layer. Finally, bias-controlled in-situ nucleation of the large-size single-crystal diamond on the iridium surface and subsequent unbiased epitaxial growth are achieved. This method solves the problem of dislocation extension at the splicing positions of homogeneous substrates, and the mosaic-spliced single-crystal diamond wafer can be reused. However, it does not address the unavoidable dislocation defects inherent in epitaxial diamond growth, such as the diamond's lattice constant... ) and iridium (lattice constant) Diamond has a large lattice mismatch of 7%, and its linear expansion coefficient is 1.1 × 10⁻⁶. -6 K -1 ) and iridium (linear expansion coefficient 7.1×10 -6 K -1 The interface generates significant internal stress, which makes the diamond epitaxial layer a brittle film, limiting the size of the synthesized layer and making further processing difficult.
[0005] The key to developing diamond technology lies not only in the growth and preparation of the diamond epitaxial layer, but also in the separation of the diamond epitaxial layer from the substrate. Only by reducing structural defects and maintaining good performance during the preparation and separation process can the synthesis of large-size diamonds be achieved. Therefore, avoiding brittle fracture in large-size diamond materials is a pressing issue that needs to be addressed. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a method for synthesizing large-size diamond crystals using chemical vapor deposition. A substrate is formed by tightly composited single-crystal silicon, SiO2 film, and TiCN film. Etching of the TiCN and SiO2 films creates buffer spaces within the substrate structure, reducing internal stress caused by differences in material expansion coefficients. Furthermore, by controlling the diamond deposition environment and heat treatment method, the bonding force between the epitaxially grown diamond and the substrate is enhanced, residual stress is reduced, and structural defects are minimized. This ensures the epitaxial growth of large-size diamonds while improving the mechanical properties of the diamond, thus preventing brittle fracture of the diamond material during synthesis and separation.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] A method for synthesizing large-size diamond crystals using chemical vapor deposition (CVD) involves using pretreated single-crystal silicon as a substrate. SiO2 and TiCN films are sequentially deposited on one side of the substrate using plasma-enhanced CVD. Then, windows arranged in a uniform array are etched into the TiCN film. The SiO2 film beneath the windows and portions of the SiO2 film between adjacent windows are removed by window etching. After cleaning, drying, and intermediate annealing, a supporting substrate is obtained. Next, a diamond transition layer is deposited on the supporting substrate using a hydrocarbon-fluorine system via plasma-enhanced CVD, followed by the deposition of a diamond epitaxial layer using a hydrocarbon system. After ultrasonic treatment, the diamond transition layer and diamond epitaxial layer are separated, and stress-relief annealing yields the large-size diamond crystal.
[0009] The above-mentioned method for synthesizing large-size diamond crystals using chemical vapor deposition specifically includes the following steps:
[0010] S1. Substrate pretreatment: The monocrystalline silicon is polished, cleaned, and dried to obtain the substrate;
[0011] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 250-350℃, maintain for 15-30 min, then introduce N2O until the pressure in the reaction chamber is 70-100 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 40-50 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a SiO2 film with a thickness of 0.6-2.4 μm under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 4-8 min;
[0012] S3. Deposition of TiCN film: Heat the reaction chamber to 500-580℃, control the pressure inside the reaction chamber to 220-300Pa, and adjust the radio frequency power applied to the substrate to 80-100W. Use TiCl4, CH4, N2, and H2 as the deposition gas source, and deposit a TiCN film with a thickness of 0.8-3.0μm under constant temperature and pressure. Stop the introduction of TiCl4, CH4, and N2, maintain the H2 plasma environment for 3-6 minutes, cool to below 100℃, and then remove the film.
[0013] S4. Etching TiCN film and SiO2 film: Photoresist is coated on TiCN film, and a pattern is formed by ultraviolet photolithography. Then, dry etching is used to etch windows in a uniform array on TiCN film. Finally, wet etching is used to remove the SiO2 film under the windows and part of the SiO2 film between adjacent windows.
[0014] S5. Cleaning, drying and intermediate annealing: After cleaning and drying the product obtained in step S4, vacuum anneal it at 250-350℃ for 30-60 min, and then cool it to room temperature in the furnace to obtain the support substrate.
[0015] S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1000-1200W, the deposition gas pressure to be 3.0-3.5kPa, and the substrate temperature to be 650-750℃, use a mixed gas of H2, CH4 and CF4 as the reaction gas source, nucleation for 15-30min under a bias voltage of -190 to -250V, then stop the bias nucleation, continue deposition for 1-1.5h, then stop introducing CF4 to form a diamond transition layer;
[0016] S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0-4.5 kPa and the substrate temperature to 850-950℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for more than 48 hours; after the required thickness for epitaxial growth is reached, stop the introduction of CH4, maintain the H2 plasma environment for 5-10 minutes, and take it out when cooled to 180-220℃;
[0017] S8. Ultrasonic treatment and separation: The product obtained in step S7 is placed in room temperature ethanol and ultrasonically treated for 20-40 minutes to separate the diamond transition layer and the diamond epitaxial layer. After removing the residual SiO2 film and TiCN film on the surface, it is cleaned and dried.
[0018] S9. Stress-relieving annealing: Place in a vacuum heating furnace and evacuate to a pressure less than 10. -2The pressure is increased to 1-3 MPa, and a mixture of CH4, H2 and N2 is introduced into the furnace. The temperature is maintained at 600-850℃ for 1-2.5 hours. Heating is then stopped, and the furnace is cooled to below 60℃ before being removed.
[0019] This invention employs a three-layer composite of monocrystalline silicon, SiO2 film, and TiCN film, resulting in strong interlayer bonding. By optimizing the structure of the supporting substrate, a buffer space is created between the TiCN film and the substrate, which helps reduce the internal stress caused by the difference in the coefficients of thermal expansion of the materials. Furthermore, intermediate annealing eliminates stress concentration in the supporting substrate and improves its impact resistance, thereby reducing the risk of warping or cracking of the supporting substrate and diamond, and also facilitating the separation of diamond from the heterogeneous substrate.
[0020] This invention controls the process parameters of plasma chemical vapor deposition to achieve a stable and dense film, which facilitates diamond nucleation and growth and reduces structural defects. During the deposition of the diamond transition layer, fluorine (F) is introduced into the vapor system, partially replacing hydrogen atoms in the microstructure with F atoms. This reduces internal stress, improves the bonding strength between the diamond transition layer and the supporting substrate, and enhances macroscopic structural stability. Simultaneously, F atoms can interact with non-diamond carbon (eroding non-diamond carbon) to maintain the active surface for diamond growth, ensuring continuous diamond growth and improving diamond toughness. After growing the diamond epitaxial layer, a CH-terminated structure is formed. Ultrasonic treatment introduces stress, partially offsetting residual stress to achieve stress balance and control. Annealing further eliminates residual stress, stabilizes the microstructure uniformity, and further improves the mechanical properties of the diamond.
[0021] To facilitate the growth of SiO2 film, TiCN film and diamond, the substrate in step S1 is selected as single-crystal silicon with (111) crystal orientation. The cleaning is performed by ultrasonic cleaning with acetone, anhydrous ethanol and pure water in sequence. Although diamond (111) has a high surface density and is prone to cracking, diamond grown in this crystal orientation has high hardness and strength. By controlling the process to improve the toughness of diamond, it is possible to achieve a comprehensive improvement in the mechanical properties of diamond.
[0022] As an intermediate layer supporting the substrate, the SiO2 film needs to effectively connect the substrate and the TiCN film. In step S2, the flow rate ratio of SiH4, N2O and N2 is 1:8 to 10:4 to 9, the flow rate of SiH4 is 20 to 25 sccm, and N2 is used as a dilution gas for SiH4. The deposition rate is controlled by controlling the ratio of SiH4, N2O and N2 so that the SiO2 film has a certain density.
[0023] In order to maintain good structure and mechanical properties of the TiCN film after etching and to facilitate the nucleation and growth of the diamond transition layer, the total flow rate of the deposition gas source in step S3 is controlled to be 300-400 sccm, and the volume percentage of TiCl4, CH4, and N2 in the deposition gas source is 1.5-2.5%, 3-5%, and 28-32%, respectively.
[0024] To achieve better etching results and ensure the supporting substrate meets structural requirements, the dry etching in step S4 is performed using gas etching with CCl4, CF2Cl2, or CF3Cl. The window is a square with a side length of 2–20 μm, and the surface area of the etched TiCN film is 40–80% of the substrate surface area. The wet etching is performed using a chemical etching solution containing HF and NH4F, and the surface area of the etched SiO2 film is 20–40% of the substrate surface area.
[0025] To better form the diamond transition layer, the total flow rate of the reaction gas source in step S6 is 330–450 sccm, and H2 carrier gas is used when CF4 is introduced. During bias nucleation, a higher C / H ratio is required, with the volume percentage of CH4 in the reaction gas source being 3.0–4.5% and the volume percentage of CF4 being 500–750 ppm. After the bias nucleation deposition is completed, the C / H ratio is reduced, with the volume percentage of CH4 in the reaction gas source being 1.0–2.5% and the volume percentage of CF4 being 500–750 ppm. To obtain a better diamond growth rate and growth effect, the total flow rate of the growth gas source in step S7 is 330–450 sccm, and the volume percentage of CH4 in the growth gas source is 1.0–2.5%.
[0026] In order to separate the diamond transition layer and the diamond epitaxial layer, step S8 involves soaking the diamond transition layer and the diamond epitaxial layer in a mixture of hydrofluoric acid and nitric acid to remove the residual TiCN film and SiO2 film on the diamond transition layer and the diamond epitaxial layer.
[0027] During stress stabilization during annealing, to further compensate for growth defects in the double-doped diamond, the volume percentage of CH4 in the CH4, H2, and N2 mixture in step S9 is 1–5%, and the volume percentage of H2 is 0.5–2.5%. To better improve the annealing effect, the stress-relief annealing in step S9 adopts a gradient heating method: under constant pressure, the temperature is first increased to 600–650℃ at a heating rate of 4–7℃ / min and held at that temperature for 25–35 min; then increased to 700–750℃ at a heating rate of 8–12℃ / min and held at that temperature for 25–35 min; finally, the temperature is increased to 800–850℃ at a heating rate of 8–12℃ / min and held at that temperature for 25–35 min.
[0028] To address the brittle fracture problem of diamond during synthesis and separation, this invention tackles both external conditions and internal factors. By selecting appropriate materials, optimizing the structure, and controlling the process of the supporting substrate, the adverse effects caused by the difference in the coefficients of thermal expansion between the supporting substrate and diamond are reduced, providing a foundation for stable diamond growth and facilitating effective diamond exfoliation. Simultaneously, by adjusting the synthesis process of the diamond transition layer and the diamond epitaxial layer, large-size diamonds are grown, and diamond performance is improved, avoiding brittle fracture. Through the synergistic effect of the supporting substrate preparation and the epitaxial growth of diamond, warping or fracture during heteroepitaxial growth and separation of diamond is avoided. Attached Figure Description
[0029] Figure 1 This invention relates to a method for synthesizing large-size diamond crystals.
[0030] Figure 2 This is the X-ray diffraction pattern of the diamond obtained in Example 1;
[0031] Figure 3 These are comparison images of the Raman spectra of diamonds obtained in Example 1, Comparative Example 2, and Comparative Example 3. Detailed Implementation
[0032] To make the technical objectives, technical solutions, and beneficial effects of the present invention clearer, the technical solutions of the present invention will be further described below in conjunction with specific embodiments. However, the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. Where no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product manual shall apply.
[0033] Example 1
[0034] Methods for synthesizing large-size diamond crystals using chemical vapor deposition, such as... Figure 1 As shown, it includes the following steps:
[0035] S1. Substrate pretreatment: Select (111) crystal orientation single crystal silicon as substrate (4 inches), polish the substrate to roughness Ra < 1 nm, use an ultrasonic cleaner to ultrasonically clean the substrate with acetone, anhydrous ethanol and pure water for 10 min each, take it out and dry it (blow dry) to obtain the substrate.
[0036] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5Pa, heat the reaction chamber to 300℃, maintain for 20 min, then introduce N2O until the pressure in the reaction chamber is 80 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 40 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a 0.8 μm thick SiO2 film under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 5 min;
[0037] The flow rate of N2O is 180 sccm, the flow rate of SiH4 is 20 sccm, and the flow rate of N2 is 160 sccm. SiH4 is introduced through N2 carrier gas, that is, N2 is used as dilution gas for SiH4.
[0038] S3, Deposition of TiCN film: The reaction chamber is heated to 540℃, the pressure inside the reaction chamber is controlled at 260Pa, and the radio frequency power applied to the substrate is adjusted to 80W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A TiCN film with a thickness of 0.8μm is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH4, and N2 is stopped, the heating is stopped, and the H2 plasma environment is maintained for 4 minutes. After cooling to below 100℃, it is taken out.
[0039] The flow rate of TiCl4 was 7.2 sccm, the flow rate of CH4 was 14.4 sccm, the flow rate of N2 was 108 sccm, and the flow rate of H2 was 230.4 sccm. TiCl4 was evaporated and then introduced with H2 as carrier gas.
[0040] S4. Etching TiCN film and SiO2 film: Photoresist is coated on TiCN film, and a pattern is formed by ultraviolet photolithography. Then, dry etching is used to etch windows (squares with a side length of 8μm) evenly arranged in an array on TiCN film. Then, wet etching is used to remove the SiO2 film below the window and part of the SiO2 film between adjacent windows.
[0041] The dry etching is performed using gas etching with CCl4, CF2Cl2, or CF3Cl, resulting in a TiCN film with a surface area of 60% of the substrate surface area. The wet etching is performed using a chemical etching with an aqueous solution containing HF and NH4F (buffered hydrofluoric acid solution, BHF), resulting in a SiO2 film with a surface area of 30% of the substrate surface area. The specific control of gas etching and chemical etching can be achieved using conventional techniques in the field and is not an innovation of this invention, so it will not be described in detail.
[0042] S5. Cleaning, drying and intermediate annealing: The product obtained in step S4 is ultrasonically cleaned with anhydrous ethanol and pure water for 10 min each, taken out and dried (blown dry), vacuum annealed at 300℃ for 40 min, and cooled to room temperature in the furnace to obtain the support substrate.
[0043] S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0044] During bias nucleation, the flow rate of pure H2 was 351.6 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm; during deposition after bias nucleation, the flow rate of pure H2 was 360 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm.
[0045] S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 168h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out when it is cooled to 200℃.
[0046] The flow rate of H2 was 383.4 sccm, and the flow rate of CH4 was 6.6 sccm.
[0047] S8. Ultrasonic treatment and separation: The product obtained in step S7 is placed in room temperature ethanol and ultrasonically treated for 30 minutes. Then, it is soaked in a mixture of hydrofluoric acid and nitric acid (soaking to separate diamond is a conventional technique in this field) to separate the diamond transition layer and the diamond epitaxial layer. After removing the residual SiO2 film and TiCN film on the surface, it is rinsed with water and dried.
[0048] S9. Stress-relieving annealing: Place in a vacuum heating furnace and evacuate to a pressure less than 10. -2The temperature is increased to 650°C at a rate of 5°C / min, and a mixture of methane, hydrogen, and nitrogen (containing 2 wt% methane and 1 wt% hydrogen) is introduced into the furnace. The pressure is maintained at 2 MPa, and the temperature is held constant for 0.5 h. Then, the temperature is increased to 750°C at a rate of 10°C / min and held constant for 0.5 h. Then, the temperature is increased to 850°C at a rate of 10°C / min and held constant for 0.5 h. After cooling to below 60°C in the furnace, the material is removed and surface polished (using existing technology, polishing to a surface roughness of <1 nm) to obtain a large-size diamond material with a thickness of 1.5 mm.
[0049] X-ray diffraction analysis was performed on the large-size diamond material obtained in Example 1, and the results are as follows: Figure 2 As shown in the spectrum, the peak positions correspond to the characteristic diffraction peaks of the diamond crystal planes (111), (220) and (311). The (111) diffraction peak is very strong and sharp, while the relative intensities of the (220) and (311) diffraction peaks are relatively small. This indicates that the growth direction of the prepared large-size diamond grains is basically the same, that is, the (111) crystal orientation is dominant.
[0050] Example 2
[0051] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 and S4-S9 of Example 1, except that steps S2 and S3 are changed as follows:
[0052] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 300℃, maintain for 20 min, then introduce N2O until the pressure in the reaction chamber is 90 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 50 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a 0.8 μm thick SiO2 film under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 5 min;
[0053] The flow rate of N2O is 200 sccm, the flow rate of SiH4 is 25 sccm, and the flow rate of N2 is 175 sccm. SiH4 is introduced through N2 carrier gas, that is, N2 is used as dilution gas for SiH4.
[0054] S3, Deposition of TiCN film: The reaction chamber is heated to 540℃, the pressure inside the reaction chamber is controlled at 280Pa, and the radio frequency power applied to the substrate is adjusted to 90W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A 0.8μm thick TiCN film is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH4, and N2 is stopped, and the H2 plasma environment is maintained for 4 minutes. Then, the temperature is turned off and cooled to below 100℃ before being taken out.
[0055] The flow rate of TiCl4 was 8 sccm, the flow rate of CH4 was 16 sccm, the flow rate of N2 was 120 sccm, and the flow rate of H2 was 256 sccm. TiCl4 was evaporated and then introduced with H2 as carrier gas.
[0056] Example 3
[0057] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 and S4-S9 of Example 1, except that steps S2 and S3 are changed as follows:
[0058] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 350℃, maintain for 20 min, then introduce N2O until the pressure in the reaction chamber is 100 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 50 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a 0.8 μm thick SiO2 film under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 5 min;
[0059] The flow rate of N2O is 200 sccm, the flow rate of SiH4 is 20 sccm, the flow rate of N2 is 180 sccm, and SiH4 is introduced through N2 carrier gas, that is, N2 is used as dilution gas for SiH4.
[0060] S3, Deposition of TiCN film: The reaction chamber is heated to 580℃, the pressure inside the reaction chamber is controlled at 300Pa, and the radio frequency power applied to the substrate is adjusted to 100W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A 0.8μm thick TiCN film is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH4, and N2 is stopped, and the H2 plasma environment is maintained for 4 minutes. Then, the temperature is turned off and cooled to below 100℃ before being taken out.
[0061] The flow rate of TiCl4 is 10 sccm, the flow rate of CH4 is 20 sccm, the flow rate of N2 is 120 sccm, and the flow rate of H2 is 250 sccm. TiCl4 is evaporated and then introduced with H2 as carrier gas.
[0062] Compared with Example 1, Examples 2 and 3 adjusted the pressure, radio frequency power, and gas flow rate, which increased the deposition rate of SiO2 film and TiCN film, and changed the density and bonding force. However, as long as steps S2 and S3 are within the defined parameter range, diamond epitaxial growth can be achieved.
[0063] Example 4
[0064] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1-S5 and S7-S9 of Example 1, except that step S6 is changed as follows:
[0065] S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0066] During bias nucleation, the flow rate of pure H2 was 355.5 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1vt%CF4) was 19.5 sccm. During deposition after bias nucleation, the flow rate of pure H2 was 363.9 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1vt%CF4) was 19.5 sccm.
[0067] Example 5
[0068] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1-S5 and S7-S9 of Example 1, except that step S6 is changed as follows:
[0069] S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0070] During bias nucleation, the flow rate of pure H2 was 346 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1vt%CF4) was 29 sccm. During deposition after bias nucleation, the flow rate of pure H2 was 354.4 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1vt%CF4) was 29 sccm.
[0071] Example 6
[0072] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1-S6, S8, and S9 of Example 1, except that step S7 is changed as follows:
[0073] S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 200h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out when it is cooled to 200℃.
[0074] The flow rate of H2 was 395 sccm, and the flow rate of CH4 was 5 sccm.
[0075] Example 7
[0076] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1-S6, S8, and S9 of Example 1, except that step S7 is changed as follows:
[0077] S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 120h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out when it is cooled to 200℃.
[0078] The flow rate of H2 was 380.5 sccm, and the flow rate of CH4 was 9.5 sccm.
[0079] Example 8
[0080] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 to S8 of Example 1, except that step S9 is changed as follows:
[0081] Stress-relief annealing: Place in a vacuum heating furnace and evacuate to a pressure less than 10. -2The furnace is heated to 600°C at a heating rate of 5°C / min, and a mixture of methane, hydrogen, and nitrogen (containing 2 wt% methane and 1 wt% hydrogen) is introduced into the furnace. The pressure is maintained at 2 MPa, and the temperature is held constant for 0.5 h. Then, the temperature is increased to 700°C at a heating rate of 10°C / min and held constant for 0.5 h. Finally, the temperature is increased to 800°C at a heating rate of 10°C / min and held constant for 0.5 h. After cooling to below 60°C in the furnace, the material is removed and surface polished (using existing technology, polishing to a surface roughness of <1 nm) to obtain a large-size diamond material with a thickness of 1.5 mm.
[0082] Example 9
[0083] The method for synthesizing large-size diamond crystals using chemical vapor deposition is the same as that in Example 1, except that the substrate in step S1 is replaced with a 6-inch substrate, resulting in a large-size diamond material with a thickness of 1.5 mm.
[0084] Comparative Example 1
[0085] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 to S8 of the technical solution in Example 1, except that step S9 is omitted, and thus includes the following steps:
[0086] S1. Substrate pretreatment: Select (111) crystal orientation single crystal silicon as substrate, polish the substrate to roughness Ra < 1nm, use an ultrasonic cleaner to ultrasonically clean the substrate with acetone, anhydrous ethanol and pure water for 10min each, take it out and dry it (blow dry) to obtain the substrate.
[0087] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 300℃, maintain for 20 min, then introduce N2O until the pressure in the reaction chamber is 80 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 40 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a 0.8 μm thick SiO2 film under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 5 min;
[0088] The flow rate of N2O is 180 sccm, the flow rate of SiH4 is 20 sccm, and the flow rate of N2 is 160 sccm. SiH4 is introduced through N2 carrier gas, that is, N2 is used as dilution gas for SiH4.
[0089] S3, Deposition of TiCN film: The reaction chamber is heated to 540℃, the pressure inside the reaction chamber is controlled at 260Pa, and the radio frequency power applied to the substrate is adjusted to 80W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A TiCN film with a thickness of 0.8μm is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH4, and N2 is stopped, the heating is stopped, and the H2 plasma environment is maintained for 4 minutes. After cooling to below 100℃, it is taken out.
[0090] The flow rate of TiCl4 was 7.2 sccm, the flow rate of CH4 was 14.4 sccm, the flow rate of N2 was 108 sccm, and the flow rate of H2 was 230.4 sccm. TiCl4 was evaporated and then introduced with H2 as carrier gas.
[0091] S4. Etching TiCN film and SiO2 film: Photoresist is coated on TiCN film, and a pattern is formed by ultraviolet photolithography. Then, dry etching is used to etch windows (squares with a side length of 8μm) evenly arranged in an array on TiCN film. Then, wet etching is used to remove the SiO2 film below the window and part of the SiO2 film between adjacent windows.
[0092] The dry etching is performed using gas etching with CCl4, CF2Cl2, or CF3Cl, resulting in a TiCN film with a surface area of 60% of the substrate surface area. The wet etching is performed using a chemical etching with an aqueous solution containing HF and NH4F (buffered hydrofluoric acid solution, BHF), resulting in a SiO2 film with a surface area of 30% of the substrate surface area. The specific control of gas etching and chemical etching can be achieved using conventional techniques in the field and is not an innovation of this invention, so it will not be described in detail.
[0093] S5. Cleaning, drying and intermediate annealing: The product obtained in step S4 is ultrasonically cleaned with anhydrous ethanol and pure water for 10 min each, taken out and dried (blown dry), vacuum annealed at 300℃ for 40 min, and cooled to room temperature in the furnace to obtain the support substrate.
[0094] S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0095] During bias nucleation, the flow rate of pure H2 was 351.6 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm; during deposition after bias nucleation, the flow rate of pure H2 was 360 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm.
[0096] S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 168h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out when it is cooled to 200℃.
[0097] The flow rate of H2 was 383.4 sccm, and the flow rate of CH4 was 6.6 sccm.
[0098] S8. Ultrasonic treatment and separation: The product obtained in step S7 is placed in room temperature ethanol and ultrasonically treated for 30 minutes. Then, it is soaked in a mixture of hydrofluoric acid and nitric acid to separate the diamond transition layer and the diamond epitaxial layer. After removing the residual SiO2 film and TiCN film on the surface, it is rinsed with water, polished, and dried.
[0099] Comparative Example 2
[0100] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1, S3, and S5-S7 of the technical solution in Comparative Example 1, except that step S2 is omitted and steps S4 and S8 (without ultrasonic treatment) are adjusted. That is, it includes the following steps:
[0101] S1. Substrate pretreatment: Select (111) crystal orientation single crystal silicon as substrate, polish the substrate to roughness Ra < 1nm, use an ultrasonic cleaner to ultrasonically clean the substrate with acetone, anhydrous ethanol and pure water for 10min each, take it out and dry it (blow dry) to obtain the substrate.
[0102] S2, Deposition of TiCN film: The reaction chamber is heated to 540℃, the pressure inside the reaction chamber is controlled at 260Pa, and the radio frequency power applied to the substrate is adjusted to 80W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A TiCN film with a thickness of 0.8μm is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH3CN, and N2 is stopped, the heating is stopped, and the H2 plasma environment is maintained for 4 minutes. After cooling to below 100℃, it is taken out.
[0103] The flow rate of TiCl4 was 7.2 sccm, the flow rate of CH4 was 14.4 sccm, the flow rate of N2 was 108 sccm, and the flow rate of H2 was 230.4 sccm. TiCl4 was evaporated and then introduced with H2 as carrier gas.
[0104] S3. Etching TiCN film: Photoresist is coated on TiCN film, a pattern is formed by ultraviolet photolithography, and then dry etching is used to etch TiCN film into windows (squares with a side length of 8μm) that are evenly arranged in an array.
[0105] The dry etching is performed by gas etching using CCl4, CF2Cl2 or CF3Cl, and the surface area of the etched TiCN film is 60% of the surface area of the substrate.
[0106] S4. Cleaning, drying and intermediate annealing: The product obtained in step S4 is ultrasonically cleaned with anhydrous ethanol and pure water for 10 min each, taken out and dried (blown dry), vacuum annealed at 300℃ for 40 min, and cooled to room temperature in the furnace to obtain the support substrate.
[0107] S5. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0108] During bias nucleation, the flow rate of pure H2 was 351.6 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm; during deposition after bias nucleation, the flow rate of pure H2 was 360 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm.
[0109] S6. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 168h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out after cooling.
[0110] The flow rate of H2 was 383.4 sccm, and the flow rate of CH4 was 6.6 sccm.
[0111] S7. Separation: Peel off the diamond transition layer and diamond epitaxial layer, rinse with water, polish and dry.
[0112] Comparative Example 3
[0113] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 and S6-S7 of the technical solution in Comparative Example 1, except that steps S2-S5 are omitted and step S8 (without ultrasonic treatment) is adjusted. Therefore, it includes the following steps:
[0114] S1. Substrate pretreatment: Select (111) crystal orientation single crystal silicon as substrate, polish the substrate to roughness Ra < 1nm, use an ultrasonic cleaner to ultrasonically clean the substrate with acetone, anhydrous ethanol and pure water for 10min each, take it out and dry it (blow dry) to obtain the substrate.
[0115] S2. Depositing a diamond transition layer: Place the substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1200W, the deposition gas pressure to be 3.0kPa, and the substrate temperature to be 700℃, use a mixed gas of H2, CH4 and CF4 (H2 carrying CF4) as the reaction gas source, nucleation for 20min under a bias voltage of -210V, then stop the bias nucleation, continue deposition for 60min, and then stop introducing CF4 (H2 carrying CF4) to form a diamond transition layer.
[0116] During bias nucleation, the flow rate of pure H2 was 351.6 sccm, the flow rate of CH4 was 15 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm; during deposition after bias nucleation, the flow rate of pure H2 was 360 sccm, the flow rate of CH4 was 6.6 sccm, and the flow rate of H2 loaded with CF4 (1 vt% CF4) was 23.4 sccm.
[0117] S3. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0 kPa and the substrate temperature to 900℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for 168h; after the epitaxial growth is completed, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out after cooling.
[0118] The flow rate of H2 was 383.4 sccm, and the flow rate of CH4 was 6.6 sccm.
[0119] S4. Separation: Peel off the diamond transition layer and diamond epitaxial layer, rinse with water, polish and dry.
[0120] Comparative Example 4
[0121] The method for synthesizing large-size diamond crystals using chemical vapor deposition follows steps S1 to S5 and S8 of the technical solution in Comparative Example 1, except that step S6 is omitted and step S7 is adjusted, which includes the following steps:
[0122] S1. Substrate pretreatment: Select (111) crystal orientation single crystal silicon as substrate, polish the substrate to roughness Ra < 1nm, use an ultrasonic cleaner to ultrasonically clean the substrate with acetone, anhydrous ethanol and pure water for 10min each, take it out and dry it (blow dry) to obtain the substrate.
[0123] S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 300℃, maintain for 20 min, then introduce N2O until the pressure in the reaction chamber is 80 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 40 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit to form a 0.8 μm thick SiO2 film under constant temperature and pressure, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 5 min;
[0124] The flow rate of N2O is 180 sccm, the flow rate of SiH4 is 20 sccm, and the flow rate of N2 is 160 sccm. SiH4 is introduced through N2 carrier gas, that is, N2 is used as dilution gas for SiH4.
[0125] S3, Deposition of TiCN film: The reaction chamber is heated to 540℃, the pressure inside the reaction chamber is controlled at 260Pa, and the radio frequency power applied to the substrate is adjusted to 80W. TiCl4, CH4, N2, and H2 are used as the deposition gas source. A 0.8μm thick TiCN film is formed by reaction deposition under constant temperature and pressure. The introduction of TiCl4, CH3CN, and N2 is stopped, the heating is stopped, and the H2 plasma environment is maintained for 4 minutes. After cooling to below 100℃, it is taken out.
[0126] The flow rate of TiCl4 was 7.2 sccm, the flow rate of CH4 was 14.4 sccm, the flow rate of N2 was 108 sccm, and the flow rate of H2 was 230.4 sccm. TiCl4 was evaporated and then introduced with H2 as carrier gas.
[0127] S4. Etching TiCN film and SiO2 film: Photoresist is coated on TiCN film, and a pattern is formed by ultraviolet photolithography. Then, dry etching is used to etch windows (squares with a side length of 8μm) evenly arranged in an array on TiCN film. Then, wet etching is used to remove the SiO2 film below the window and part of the SiO2 film between adjacent windows.
[0128] The dry etching is performed using gas etching with CCl4, CF2Cl2, or CF3Cl, resulting in a TiCN film with a surface area of 60% of the substrate surface area. The wet etching is performed using a chemical etching with an aqueous solution containing HF and NH4F (buffered hydrofluoric acid solution, BHF), resulting in a SiO2 film with a surface area of 30% of the substrate surface area. The specific control of gas etching and chemical etching can be achieved using conventional techniques in the field and is not an innovation of this invention, so it will not be described in detail.
[0129] S5. Cleaning, drying and intermediate annealing: The product obtained in step S4 is ultrasonically cleaned with anhydrous ethanol and pure water for 10 min each, taken out and dried (blown dry), vacuum annealed at 300℃ for 40 min, and cooled to room temperature in the furnace to obtain the support substrate.
[0130] S6. Growth of Diamond Epitaxial Layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to 1200W, control the deposition gas pressure to 4.0kPa, and the substrate temperature to 900℃, use the mixed gas of H2 and CH4 as the growth gas source, nucleate for 20min under a bias voltage of -210V, then stop the bias nucleation, continue to deposit to the required thickness, stop the introduction of CH4, maintain the H2 plasma environment for 10min, and take it out when cooled to 200℃;
[0131] During bias nucleation, the flow rate of pure H2 was 375 sccm and the flow rate of CH4 was 15 sccm; during deposition after bias nucleation, the flow rate of pure H2 was 383.4 sccm and the flow rate of CH4 was 6.6 sccm.
[0132] S7. Ultrasonic treatment and separation: The product obtained in step S6 is placed in room temperature ethanol and ultrasonically treated for 30 minutes. Then, it is soaked in a mixture of hydrofluoric acid and nitric acid to separate the diamond transition layer and the diamond epitaxial layer. After removing the residual SiO2 film and TiCN film on the surface, it is rinsed with water, polished, and dried.
[0133] Raman spectroscopy analysis was performed on the diamond samples obtained in Example 1 and Comparative Examples 2 and 3. The results are as follows: Figure 3 As shown in the comparison of the spectra, the Raman scattering peak of the diamond sample obtained in Example 1 is located at 1332 cm⁻¹. -1 At the location, with diamond crystal sp 3The standard characteristic peaks of the bonds are consistent. The Raman scattering peaks of Comparative Example 2 and Comparative Example 3 are shifted to the right, which may be due to the internal stress caused by the difference in thermal expansion coefficients. Diamond has a small thermal expansion coefficient. When the synthesized sample is restored to room temperature (without annealing treatment), the diamond film is subjected to compressive stress, which causes the Raman scattering peak to shift in the direction of increasing wavenumber.
[0134] The mechanical properties of the diamond samples grown in Examples 1, 4-9 and Comparative Examples 1-4 were tested, and the results are shown in Table 1.
[0135] Table 1 Mechanical properties of diamond samples obtained from the examples and comparative examples
[0136] sample Hardness / GPa Fracture strength / MPa <![CDATA[Fracture toughness / MPa·m 0.5 > Example 1 41.3 1145 17.5 Example 4 40.6 1089 15.6 Example 5 42.2 1152 17.7 Example 6 47.8 1190 18.0 Example 7 38.5 1112 16.9 Example 8 41.0 1148 17.4 Example 9 40.9 1131 17.6 Comparative Example 1 47.4 781 8.7 Comparative Example 2 49.3 578 7.1 Comparative Example 3 50.5 605 6.9 Comparative Example 4 45.3 658 8.2
[0137] As shown in Table 1, the large-size diamonds prepared by this invention have a hardness of up to 47.8 GPa, a fracture strength of up to 1190 GPa, and a fracture toughness of up to 18.0 MPa·m. 0.5 During the growth of the diamond epitaxial layer, the hardness, fracture strength, and fracture toughness all decreased slightly with the increase of C content. During the deposition of the diamond transition layer, the hardness, fracture strength, and fracture toughness all increased slightly with the increase of F content, possibly because a small amount of F in the system has the effect of refining diamond grains. Comparative Example 1 did not undergo annealing treatment, and its fracture strength and fracture toughness decreased significantly, indicating that annealing treatment has a promoting effect on compositional uniformity and defect compensation, and can significantly improve mechanical properties. Comparative Example 4 did not deposit a diamond transition layer, and its hardness, fracture strength, and fracture toughness all decreased. Although the hardness of Comparative Examples 2 and 3 was better than that of Examples 1-9, due to the difference in the coefficient of thermal expansion between the substrate and diamond, the fracture strength and fracture toughness of the separated samples decreased significantly compared with the samples of the examples, making it difficult to synthesize larger diamond crystals.
[0138] In summary, this invention improves the mechanical properties (fracture strength and fracture toughness) of diamond through material selection, structural optimization, and process control, which helps to achieve the growth of large-size diamonds and avoids brittle fracture.
[0139] The above embodiments merely illustrate several implementation methods of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
[0140] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for synthesizing large-size diamond crystals using chemical vapor deposition, characterized in that: Using pretreated single-crystal silicon as a substrate, SiO2 and TiCN films are sequentially deposited on one side of the substrate using plasma-enhanced chemical vapor deposition (PECVD). Then, windows arranged in a uniform array are etched onto the TiCN film. The SiO2 film below the windows and parts of the SiO2 film between adjacent windows are removed by window etching. After cleaning, drying, and intermediate annealing, a supporting substrate is obtained. Next, a diamond transition layer is deposited on the supporting substrate using a hydrocarbon-fluorine system via PCVD, followed by the deposition and growth of a diamond epitaxial layer using a hydrocarbon system. After ultrasonic treatment, the diamond transition layer and diamond epitaxial layer are separated, and after stress-relief annealing, a large-size diamond crystal is obtained. Specifically, it includes the following steps: S1. Substrate pretreatment: The monocrystalline silicon is polished, cleaned, and dried to obtain the substrate; S2. Depositing SiO2 film: The pretreated substrate is placed in an RF plasma chemical vapor deposition apparatus, and the vacuum is evacuated to a pressure less than 10. -5 Pa, heat the reaction chamber to 250~350℃, maintain for 15~30 min, then introduce N2O until the pressure in the reaction chamber is 70~100 Pa, turn on the radio frequency source and adjust the radio frequency power applied to the substrate to 40~50 W, while maintaining the introduction of N2O, introduce SiH4 and N2, N2O and SiH4 react and deposit under constant temperature and pressure to form a SiO2 film with a thickness of 0.6~2.4 μm, stop the introduction of N2O and SiH4, and maintain the N2 plasma environment for 4~8 min; S3. Deposition of TiCN film: Heat the reaction chamber to 500~580℃, control the pressure inside the reaction chamber to 220~300 Pa, and adjust the radio frequency power applied to the substrate to 80~100 W. Use TiCl4, CH4, N2, and H2 as the deposition gas source, and deposit a TiCN film with a thickness of 0.8~3.0 μm under constant temperature and pressure. Stop the introduction of TiCl4, CH4, and N2, maintain the H2 plasma environment for 3~6 min, cool to below 100℃, and then take it out. S4. Etching TiCN film and SiO2 film: Photoresist is coated on TiCN film, and a pattern is formed by ultraviolet photolithography. Then, dry etching is used to etch windows in a uniform array on TiCN film. Finally, wet etching is used to remove the SiO2 film under the windows and part of the SiO2 film between adjacent windows. S5. Cleaning, drying and intermediate annealing: After cleaning and drying the product obtained in step S4, vacuum anneal it at 250~350℃ for 30~60 min, and then cool it to room temperature in the furnace to obtain the support substrate. S6. Depositing a diamond transition layer: Place the supporting substrate in a microwave plasma chemical vapor deposition apparatus and evacuate to a pressure less than 10. -5 Pa, turn on the microwave excitation source and introduce H2, control the microwave power to be 1000~1200 W, the deposition gas pressure to be 3.0~3.5 kPa, and the substrate temperature to be 650~750℃, use a mixed gas of H2, CH4 and CF4 as the reaction gas source, nucleation for 15~30 min under a bias voltage of -190~-250 V, then stop the bias nucleation, continue deposition for 1~1.5 h, and then stop introducing CF4 to form a diamond transition layer; S7. Growth of diamond epitaxial layer: Keep the microwave power constant, control the deposition gas pressure to 4.0~4.5 kPa and the substrate temperature to 850~950℃, use a mixture of H2 and CH4 as the growth gas source, and continue to grow diamond epitaxially for more than 48 hours; after the required thickness for epitaxial growth is reached, stop the introduction of CH4, maintain the H2 plasma environment for 5~10 min, and take it out when cooled to 180~220℃; S8. Ultrasonic treatment and separation: Place the product obtained in step S7 in room temperature ethanol and ultrasonically treat it for 20~40 min to separate the diamond transition layer and diamond epitaxial layer. After removing the residual SiO2 film and TiCN film on the surface, clean and dry it. S9. Stress-relieving annealing: Place in a vacuum heating furnace and evacuate to a pressure less than 10. -2 Start heating at 1-3 MPa and introduce a mixture of CH4, H2, and N2 into the furnace. Maintain the pressure at 600-850℃ for 1-2.5 hours, then stop heating and remove the furnace after it cools to below 60℃.
2. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: In step S2, the flow rate ratio of SiH4, N2O and N2 is 1:8~10:4~9, and the flow rate of SiH4 is 20~25 sccm.
3. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: The total flow rate of the deposition gas source in step S3 is 300~400 sccm, and the volume percentage of TiCl4 in the deposition gas source is 1.5~2.5%, the volume percentage of CH4 is 3~5%, and the volume percentage of N2 is 28~32%.
4. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: In step S6, the total flow rate of the reaction gas source is 330~450 sccm, and H2 carrier gas is used when CF4 is introduced. During bias nucleation, the volume percentage of CH4 in the reaction gas source is 3.0~4.5%, and the volume percentage of CF4 is 500~750 ppm. When deposition is completed after bias nucleation, the volume percentage of CH4 in the reaction gas source is 1.0~2.5%, and the volume percentage of CF4 is 500~750 ppm.
5. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: The total flow rate of the growth gas source in step S7 is 330~450 sccm, and the volume percentage of CH4 in the growth gas source is 1.0~2.5%.
6. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: In the mixed gas of CH4, H2 and N2 mentioned in step S9, the volume percentage of CH4 is 1~5% and the volume percentage of H2 is 0.5~2.5%.
7. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 6, characterized in that, In step S9, stress-relief annealing employs a gradient heating method: under constant pressure, the temperature is first increased to 600-650℃ at a heating rate of 4-7℃ / min and held at that temperature for 25-35 min; then increased to 700-750℃ at a heating rate of 8-12℃ / min and held at that temperature for 25-35 min; finally, the temperature is increased to 800-850℃ at a heating rate of 8-12℃ / min and held at that temperature for 25-35 min.
8. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to claim 1, characterized in that: In step S4, the dry etching is performed by gas etching using CCl4, CF2Cl2, or CF3Cl. The window is a square with a side length of 2-20 μm, and the surface area of the etched TiCN film is 40-80% of the substrate surface area. The wet etching is performed by chemical etching using an aqueous solution containing HF and NH4F, and the surface area of the etched SiO2 film is 20-40% of the substrate surface area. In step S8, the separation of the diamond transition layer and the diamond epitaxial layer is performed by immersion in a mixture of hydrofluoric acid and nitric acid.
9. The method for synthesizing large-size diamond crystals using chemical vapor deposition according to any one of claims 1 to 8, characterized in that: The substrate selected in step S1 is a (111) oriented monocrystalline silicon.
Citation Information
Patent Citations
A method for splicing and growing large-size single-crystal diamond epitaxial wafers
CN110079860B
A method for vertically splicing to prepare large-size CVD diamonds and for cutting them.
CN110230091B
A method for high-quality, large-size single-crystal diamond epitaxial growth
CN111206280B
Substrate for realizing heteroepitaxial growth of large-size monocrystal diamond and preparation method thereof
CN104499047A
Secondary epitaxy method for preparing high-quality diamond single crystal by adopting nanostructure
CN110863243A