A method for collaboratively treating chromium-containing hazardous waste and waste glass
By reducing and calcining chromium-containing hazardous waste with ferrous sulfate, and melting it with palygorskite and waste glass to form spinel and network structures, the pollution problem of chromium-containing waste is solved and harmless disposal and resources are achieved. Chemical utilization significantly reduces the toxicity and migration of chromium.
Patent Information
- Application Number
- CN202310371894.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Existing technology cannot effectively handle hazardous waste containing chromium, resulting in soil and groundwater contamination, and waste glass is difficult to decompose, making it impossible to achieve complete harmlessness and resource utilization of chromium-containing waste.
By mixing chromium-containing hazardous waste with ferrous sulfate for reduction and calcination, then mixing with palygorskite and waste glass powder for melting treatment, and quenching with water to form (Mg·Fe)(Cr·Al)2O4 type spinel, Fix chromium and form a network structure to achieve structural solidification of chromium.
It achieves complete harmless disposal of hazardous waste containing chromium, reduces the toxicity and migration of chromium, and converts the treated water quenching slag into glass that can be used for building materials, realizing resource utilization and reducing the leaching toxicity of chromium. More than 70%.
Smart Images

Figure CN116371897B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for resource treatment of chromium-containing hazardous waste, in particular to a method for collaboratively treating chromium-containing hazardous waste and waste glass, and belongs to the field of harmless treatment and resource treatment of heavy metal waste. Background Art
[0002] Chromium-containing hazardous waste is a type of highly toxic and carcinogenic waste generated during industrial production. At present, a large amount of chromium-containing solid waste generated by enterprises has not been safely disposed of, but has been piled up in the factory area for a long time, causing serious pollution to the soil and groundwater. At present, the main treatment methods for chromium-containing hazardous waste are detoxification and solidification / stabilization, but they still need to be safely landfilled in the end, and the purpose of completely harmless and resource-based chromium-containing hazardous waste cannot be achieved. In the prior art (application number: 2016111122800), chromium-containing waste residues are treated by adding acid, reducing agent, adjusting pH to alkaline, adding flocculants and curing agents. This method has many steps, complicated operation, and requires long-term maintenance.
[0003] The main components of waste glass are silicon dioxide, calcium silicate and sodium silicate, and their chemical properties are very stable. The silicon dioxide in it is difficult to decompose naturally. Compared with white pollution mainly composed of plastic waste, waste glass products are even more difficult to decompose in the natural environment and cannot be degraded in landfills. Some of them even contain heavy metals such as zinc and copper, which will pollute the soil and groundwater. The silicon dioxide, calcium silicate and sodium silicate in waste glass are the chemical components that are in short supply in the melting process of chromium-containing hazardous waste. Summary of the invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for the coordinated treatment of chromium-containing hazardous wastes and waste glass.
[0005] Technical solution: To solve the above technical problems, the present invention provides a method for co-processing chromium-containing hazardous waste and waste glass, comprising the following steps:
[0006] (1) uniformly mixing chromium-containing hazardous waste powder and ferrous sulfate, and performing reduction calcination to obtain a calcined product;
[0007] (2) mixing the calcined product of step (1) with palygorskite powder and waste glass powder to obtain a secondary mixed material;
[0008] (3) Melting the secondary mixed material in step (2), quenching with water, and obtaining water-quenched slag.
[0009] Wherein, the moisture content of the chromium-containing hazardous waste powder in step (1) is 0% to 3%.
[0010] Preferably, the moisture content of the chromium-containing hazardous waste powder in step (1) is 0.4% to 3%.
[0011] Wherein, the dry basis mass ratio of the chromium-containing hazardous waste powder to ferrous sulfate in step (1) is 80-90:10-20.
[0012] The reducing gas used in the reduction calcination in step (1) is carbon monoxide, the calcination temperature is 800-1150° C., and the calcination time is 30-240 min. The reducing gas can reduce part of the oxidized highly toxic hexavalent chromium, while inhibiting the oxidation of trivalent chromium to hexavalent chromium, thereby improving the curing effect of chromium.
[0013] Wherein, the moisture content of the palygorskite powder in step (2) is 0% to 3%, and the moisture content of the waste glass powder is 0% to 3%.
[0014] Preferably, the chromium-containing hazardous waste powder in step (1) and the palygorskite powder and waste glass powder in step (2) are all obtained by passing through a 200-mesh sieve. Under this condition, the chromium-containing hazardous waste powder, palygorskite powder and waste glass powder obtained have high reactivity.
[0015] The dry mass ratio of the calcined product to the palygorskite powder and the waste glass powder in step (2) is 10-50:10-30:35-80, which effectively ensures the formation of vitrified water-quenched slag.
[0016] Preferably, the dry mass ratio of the calcined product to the palygorskite powder and the waste glass powder in step (2) is 10-50:10-15:35-80.
[0017] Wherein, the melting temperature in step (3) is 1200-1600° C. and the melting time is 15-60 minutes, so that the vitrification process of the raw materials proceeds smoothly.
[0018] Wherein, the water temperature for water quenching in step (3) is 5 to 30° C., the water-to-slag ratio for water quenching is 10 to 15:1, and the water quenching time is 1 to 5 minutes.
[0019] Preferably, the water temperature used for the water quenching in step (3) is 10 to 30°C.
[0020] The principle of the invention is as follows: the invention adds ferrous sulfate to carry out reductive calcination of chromium-containing hazardous wastes, so that hexavalent chromium components such as dichromate in the chromium-containing hazardous wastes react with ferrous ions to undergo a reductive reaction, and the hexavalent chromium components with strong toxicity and mobility are converted into trivalent chromium components with greatly reduced toxicity and mobility, thereby achieving detoxification of the chromium-containing hazardous wastes; then the trivalent chromium components and iron components in the detoxified chromium-containing hazardous wastes react with palygorskite, magnesium components and silicon components in waste glass in a high-temperature melting process to form (Mg·Fe)(Cr·Al)2O4 type spinel, thereby achieving structural fixation of chromium; at the same time, sodium oxide and calcium oxide in the waste glass will be conducive to reducing the temperature and time of melt vitrification; silicon dioxide in the waste glass can inhibit the oxidation of trivalent chromium components in the melting process, thereby ensuring the smooth progress of the chromium structural fixation reaction; and after water quenching after melting, the silicon oxygen components will form a network structure, network wrap the structural solidification components, thereby achieving enhanced solidification of chromium, thereby achieving complete harmless disposal of the chromium-containing hazardous wastes. The water-quenched slag has no hazardous properties and the glass content reaches more than 90%, so it can be used as building materials, realizing the resource utilization of chromium-containing hazardous waste and waste glass.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0022] 1. The present invention is the first to synergize the treatment of chromium-containing hazardous waste and waste glass. By combining reductive calcination detoxification, molten structure solidification, and water quenching vitrification treatment, the chemical properties of the components in chromium-containing waste slag, ferrous sulfate, palygorskite and waste glass are fully utilized to achieve the enhanced solidification of chromium-containing hazardous waste and the resource utilization of chromium-containing hazardous waste and waste glass.
[0023] 2. Reductive calcination can reduce part of the oxidized highly toxic hexavalent chromium and inhibit the oxidation of trivalent chromium to hexavalent chromium. Hexavalent chromium is more toxic and mobile than trivalent chromium. Reductive calcination can promote the formation of (Mg·Fe)(Cr·Al)2O4 spinel in the melting process and improve the structural solidification of chromium, which can greatly reduce the toxicity of chromium leaching in water-quenched slag.
[0024] 3. After the chromium-containing hazardous waste is treated by reductive calcination and melt vitrification, the silicon-oxygen components will form a network structure, which will wrap the structural solidification components, and the solidification effect of chromium in the water-quenched slag will be enhanced. The test results show that the leaching toxicity of chromium in the water-quenched slag after reductive calcination and melt vitrification is reduced by more than 70% compared with single reductive calcination or melt vitrification. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0027] The chromium-containing hazardous materials were taken from Suzhou Roca Sanitary Ware (Suzhou) Co., Ltd., and its chemical composition was SiO2 3.53%, Al2O3 16.90%, Fe2O3 1.19%, MgO 0.18, CaO 1.86%, Na2O 2.91%, TiO2 0.61%, ZnO 3.38%, CuO 6.08%, SO3 17.9%, NiO 2.46, Cr2O3 42.9%, PbO 0.01%, P2O5 0.04, and Cl 0.05%.
[0028] The palygorskite was taken from a attapulgite clay mine in Jiangsu. The specific composition is: SiO2 58.05%, MgO 11.03%, Al2O3 9.55%, Fe2O3 5.20%, CaO 1.19%, K2O 1.13%, TiO2 0.43%, MnO 0.61%, Na2O0.07%, and loss on ignition 12.74%.
[0029] Waste glass was taken from domestic waste collection bins, and its chemical composition was: SiO2 68.39%, CaO 10.87%, Na2O11.15%, K2O 1.52%, Fe2O3 2.21%, BaO 0.55%, MgO 1.78%, Al2O3 2.83%, SO3 0.31%, and Cr2O3 0.39%.
[0030] Example 1
[0031] The chromium-containing hazardous waste, palygorskite and waste glass are dried respectively to reduce the moisture content of the chromium-containing hazardous waste, palygorskite and waste glass from 45%, 20% and 10% to 3% respectively, and the dried chromium-containing hazardous waste, palygorskite and waste glass are finely ground by a rod mill, and fine-grained materials are obtained through a 200-mesh sieve; 50g of chromium-containing hazardous waste is mixed with ferrous sulfate at a dry basis mass ratio of 90:10 to obtain a mixed material; the mixed material is added to a tubular furnace for reduction calcination, the reducing gas is carbon monoxide, the calcination temperature is 800°C, and the calcination time is 240 minutes. All the calcined products obtained by calcination are mixed with palygorskite and waste glass at a dry basis mass ratio of 10:10:80 to obtain a secondary mixed material, and melted in a high-temperature furnace at a melting temperature of 1600°C and a melting time of 15 minutes. After the melting is completed, water quenching is performed to obtain water-quenched slag A1. Among them, the water temperature in the water quenching is 10°C, the water-slag ratio is 10:1, and the water quenching time is 5 minutes.
[0032] The water-quenched slag was analyzed by X-ray diffraction, and the results showed that the glass content of the water-quenched slag A1 was 96%. At the same time, the heavy metal leaching toxicity of the water-quenched slag under severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested by the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007). The leaching concentration of hexavalent chromium in the water-quenched slag A1 was 0.12±0.02mg / L, which was lower than the environmental threshold, achieving the complete harmless disposal of chromium-containing hazardous wastes, and the water-quenched slag can be used as a resource.
[0033] Example 2
[0034] The chromium-containing hazardous waste, palygorskite and waste glass were dried respectively, and the moisture content of the chromium-containing hazardous waste, palygorskite and waste glass was reduced from 45%, 20% and 10% to 2% respectively; the dried chromium-containing hazardous waste, palygorskite and waste glass were finely ground by a rod mill, and fine-grained materials were obtained through a 200-mesh sieve; 50g of chromium-containing hazardous waste was mixed with ferrous sulfate at a dry basis mass ratio of 85:15, and the mixed material was added to a tube furnace for reduction calcination, the reducing gas was carbon monoxide, the calcination temperature was 1000℃, and the calcination time was 120 minutes. All the calcined products obtained by calcination were mixed with palygorskite and waste glass at a dry basis mass ratio of 30:30:40 to obtain a secondary mixed material, and melted in a high-temperature furnace at a melting temperature of 1400℃ and a melting time of 35 minutes. After the melting, water quenching was performed to obtain water-quenched slag B1. Among them, the temperature of the water for water quenching was 5℃, the water-slag ratio for water quenching was 13:1, and the water quenching time was 4 minutes.
[0035] After testing, the glass content of water-quenched slag B1 is 98%. At the same time, the heavy metal leaching toxicity of water-quenched slag in severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested using the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007). The leaching concentration of hexavalent chromium in water-quenched slag B1 is 0.23±0.01mg / L, which is lower than the environmental threshold, achieving complete harmless disposal of chromium-containing hazardous waste.
[0036] Example 3
[0037] The chromium-containing hazardous waste, palygorskite and waste glass were dried respectively to reduce the moisture content of the chromium-containing hazardous waste, palygorskite and waste glass from 45%, 20% and 10% to 0.4% respectively; the dried chromium-containing hazardous waste, palygorskite and waste glass were finely ground by a rod mill and passed through a 200-mesh sieve to obtain fine-grained materials; 50g of chromium-containing hazardous waste was evenly mixed with ferrous sulfate at a dry basis mass ratio of 80:20, and the mixed material was added to a tubular furnace for reduction calcination, the reducing gas was carbon monoxide, the calcination temperature was 1150°C, and the calcination time was 30 minutes. All the calcined products obtained by calcination were evenly mixed with palygorskite and waste glass at a dry basis mass ratio of 50:15:35 to obtain a secondary mixed material, and melted in a high-temperature furnace at a melting temperature of 1200°C and a melting time of 60 minutes. After the melting was completed, water quenching was performed to obtain water-quenched slag C3. The temperature of the water used for water quenching is 30°C, the water-to-slag ratio of water quenching is 15:1, and the water quenching time is 1 minute.
[0038] After testing, the glass content of water-quenched slag C3 is 95%. At the same time, the heavy metal leaching toxicity of water-quenched slag under severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested using the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid Nitric Acid Method" (HJ / T299-2007). The leaching concentration of hexavalent chromium in water-quenched slag C3 was 0.18±0.01mg / L, which was lower than the environmental threshold, achieving complete harmless disposal of chromium-containing hazardous waste, and the water-quenched slag can be utilized as a resource.
[0039] Comparative Example 1
[0040] According to the method of Example 1, ferrous sulfate was replaced by ferrous chloride, and other conditions remained unchanged. The obtained water-quenched slag had a glass content of 90%. At the same time, the heavy metal leaching toxicity of the water-quenched slag under a severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested using the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007). The leaching concentration of hexavalent chromium in the water-quenched slag was 6.51±0.03 mg / L, which was higher than the environmental threshold and still had hazardous characteristics.
[0041] Comparative Example 2
[0042] According to the method of Example 1, palygorskite was replaced by MgO, and other conditions remained unchanged. The obtained water-quenched slag had a glass content of 88%. At the same time, the heavy metal leaching toxicity of the water-quenched slag under a severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested using the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007). The leaching concentration of hexavalent chromium in the water-quenched slag was 17.42±0.02 mg / L, which was higher than the environmental threshold and still had hazardous characteristics.
[0043] Comparative Example 3
[0044] According to the method of Example 1, water-quenched slag was prepared under different raw material ratios, moisture contents of chromium-containing hazardous waste, palygorskite and waste glass, calcination conditions and melting conditions. The heavy metal leaching toxicity of the water-quenched slag under severe corrosion environment (salt corrosion + freeze-thaw cycle for 60 days) was tested by the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007). The results are shown in Table 1.
[0045] Table 1
[0046]
[0047]
[0048]
[0049] It can be seen that the leaching concentration of hexavalent chromium in the water-quenched slag obtained in Comparative Example 3 is higher than the environmental threshold and still has hazardous characteristics.
Claims
1. A method for co-processing chromium-containing hazardous waste and waste glass, characterized in that: The following steps are involved: (1) uniformly mixing chromium-containing hazardous waste powder and ferrous sulfate, reducing and calcining to obtain a calcined product; the dry weight ratio of the chromium-containing hazardous waste powder to the ferrous sulfate is 80-90:10-20; the reducing gas for the reduction calcination is carbon monoxide, the calcination temperature is 800-1150° C., and the calcination time is 30-240 min; (2) mixing the calcined product of step (1) with palygorskite powder and waste glass powder to obtain a secondary mixed material; the dry basis mass ratio of the calcined product to the palygorskite powder and the waste glass powder is 10-50:10-30:35-80; (3) Melting the secondary mixed material in step (2), quenching with water, and obtaining water-quenched slag.
2. The method according to claim 1, characterized in that The moisture content of the chromium-containing hazardous waste powder in step (1) is 0% to 3%.
3. The method according to claim 1, characterized in that In step (2), the moisture content of the palygorskite powder is 0% to 3%, and the moisture content of the waste glass powder is 0% to 3%.
4. The method according to claim 1, characterized in that: The melting temperature in step (3) is 1200-1600° C., and the melting time is 15-60 minutes.
5. The method according to claim 1, characterized in that The water temperature for water quenching in step (3) is 5-30° C., the water-to-slag ratio for water quenching is 10-15:1, and the water quenching time is 1-5 minutes.
6. The method according to claim 1, characterized in that The moisture content of the chromium-containing hazardous waste powder in step (1) is 0.4% to 3%.
7. The method according to claim 1, characterized in that The dry weight ratio of the calcined product to the palygorskite powder and the waste glass powder in step (2) is 10-50:10-15:35-80; and the water temperature for the water quenching in step (3) is 10-30°C.
Citation Information
Patent Citations
Method for strengthening and solidifying chromium in chromium-containing waste
CN109500046A
Harmless treatment method for treating incineration fly ash through cooperative treatment of chromium slag
CN110586612A
Fixation and stabilization of chromium in contaminated materials
US5397478A