A coal-water slurry additive using papermaking black liquor as raw material and preparation method thereof

By carrying out sulfonation and cross-linking reactions on papermaking black liquor, efficient coal-water slurry additives are prepared, which solves the problems of poor effectiveness of traditional additives and waste of resources, and achieves the high efficiency, environmental protection and economic properties of coal-water slurry additives.

CN116376608BActive Publication Date: 2024-10-11SHANGHAI CHANGFA NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310012007.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-10-11
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

Existing technology fails to effectively utilize waste slurry from the papermaking industry, resulting in resource waste and environmental pollution. Moreover, the use of traditional coal-water slurry additives is not effective and requires a large amount of additives and auxiliary additives.

Method used

Using papermaking black liquor as raw material, a coal-water slurry additive is prepared through sulfonation reaction, cross-linking reaction and partial graft copolymerization reaction. After adding sulfonating agent, catalyst and cross-linking agent, it undergoes specific temperature and insulation treatment. Generate efficient coal water slurry additives.

Benefits of technology

The coal-water slurry additive has a wide range of use alone, a small amount of addition, good stability and fluidity, reduces production costs, and meets the requirements of environmental protection and efficient resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004252525870000031
    Figure GDA0004252525870000031
  • Figure GDA0004252525870000041
    Figure GDA0004252525870000041
  • Figure GDA0004252525870000042
    Figure GDA0004252525870000042
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a water-coal slurry additive from papermaking black liquor and a preparation method thereof, and the specific steps are as follows: (1) 100 parts by mass (dry weight) of papermaking black liquor are heated to 30-70°C, 10-20 parts by mass of a sulfonating agent are added and stirred evenly, then the temperature is continued to be raised to 70-100°C, and the mixture is kept warm for 30-120 minutes; (2) the mixture is cooled to 40-80°C, 5-10 parts by mass of a catalyst and 5-10 parts by mass of a cross-linking agent are added, the temperature is raised to 80-110°C, and the mixture is kept warm for 10-90 minutes; (3) the mixture is cooled to 20-50°C, 5-10 parts by mass of a catalyst are added, and the feed liquid is dried to obtain a water-coal slurry additive having a solid content of 85-100%. The additive is applied to the water-coal slurry industry, can effectively improve the concentration and stability of the water-coal slurry, reduce the transportation cost of the water-coal slurry, and thus improve production efficiency. In addition, this product mainly uses papermaking waste liquid, reduces energy consumption and has low manufacturing costs, has social significance for energy conservation and emission reduction, and the preparation method is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of coal-water slurry additives, and in particular relates to a coal-water slurry additive using papermaking black liquor as a raw material and a preparation method thereof. Background Art

[0002] Coal-water slurry is a new type of coal-based liquid fuel that emerged in the 1970s. It is made of 65% coal, 34% water and 1% chemical additives through a certain process flow. It has low ash and sulfur content, low flame center temperature during combustion, high combustion efficiency, and low smoke, SO2 and NO X The emission is lower than that of oil and coal. Based on long-term energy strategy considerations, many countries have conducted research, development and reserve of coal-to-oil fuel technology, and have achieved commercial use.

[0003] At present, the main source of papermaking black liquor is papermaking waste pulp. Most of the papermaking black liquor is burned after alkali recovery, which not only causes serious environmental pollution, but also causes a significant waste of resources. Therefore, effectively utilizing papermaking waste liquid and developing corresponding water-coal slurry additive products can not only improve the cost-effectiveness of water-coal slurry dispersants, but also have obvious economic benefits, environmental benefits and social benefits. Summary of the invention

[0004] To achieve the above objectives, the present invention provides the following solutions.

[0005] A coal-water slurry additive using papermaking black liquor as raw material and a preparation method thereof, the specific steps are as follows:

[0006] (1) heating 100 parts by weight (dry weight) of papermaking black liquor to 30-70° C., adding 10-20 parts by weight of a sulfonating agent and stirring evenly, then continuing to heat to 70-100° C. and keeping the temperature for 30-120 minutes;

[0007] (2) cooling to 40-80° C., adding 5-10 parts by weight of a catalyst and 5-10 parts by weight of a cross-linking agent, heating to 80-110° C., and keeping warm for 10-90 minutes;

[0008] (3) Cooling the mixture to 20-50° C., adding 5-10 parts by weight of a catalyst, and drying the mixture to obtain a water-coal slurry additive having a solid content of 85-100%.

[0009] Preferably, the papermaking black liquor comprises an aqueous solution of papermaking black liquor dry powder or liquid papermaking black liquor; more preferably, in the aqueous solution of papermaking black liquor dry powder, the mass ratio of papermaking black liquor dry powder to water is 1:2-4.

[0010] Optimally, in the aqueous solution of the papermaking black liquor dry powder, the mass ratio of the papermaking black liquor dry powder to water is 1:3.

[0011] Preferably, the sulfonating agent includes one or more of formaldehyde, paraformaldehyde, and glyoxal.

[0012] Preferably, the cross-linking agent includes one or more of maleic anhydride, methyl methacrylate, and acrylonitrile.

[0013] Preferably, the catalyst includes one or more of hydrogen peroxide, sodium persulfate, and liquid alkali.

[0014] Preferably, in step (1), the temperature before adding the sulfonating agent is 50-70° C., and the insulation time after adding the sulfonating agent is 50-70 minutes.

[0015] Preferably, in step (2), the temperature before and after adding the catalyst and the cross-linking agent is 60-80° C. and 85-105° C. respectively, and the insulation time is 10-30 minutes.

[0016] Preferably, in step (3), the temperature is lowered to 30-45°C.

[0017] Preferably, in step (3), the drying is carried out by spray drying.

[0018] In this scheme, the first step is basically a sulfonation reaction, and the second step is a cross-linking reaction and a partial graft copolymerization reaction, thereby generating a more complex hydrophilic molecular structure.

[0019] The advantages of the present invention compared to the prior art are as follows:

[0020] 1. As for traditional water-coal slurry, commonly used water-coal slurry additives include naphthalene sulfonate polymer, sodium polystyrene sulfonate, sodium lignin sulfonate, etc., and the addition amount is about 0.5%-1%. Most additives are not effective when used alone, and some stabilizers and other auxiliary additives need to be added. This product has the characteristics of a wide range of single use, small addition amount, good stability of water-coal slurry products, good fluidity and low price.

[0021] 2. The dry powder and liquid black liquor used in the present invention are directly provided by papermaking enterprises and can be directly used for experimental reactions without any treatment, thus meeting the production requirements of workshops. In addition, the use of black liquor in this process has made certain contributions to environmental protection and high-value utilization.

[0022] 3. Finally, the product produced by this process has good application performance, which shows that this process can provide corresponding help for the optimization of water-coal slurry additives in the later stage. DETAILED DESCRIPTION

[0023] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0024] Example 1

[0025] A coal-water slurry additive using papermaking black liquor as raw material and a preparation method thereof, the specific steps are as follows:

[0026] (1) Add an aqueous solution of papermaking black liquor powder (100 g of papermaking black liquor powder and 400 g of deionized water) to the bottom of a kettle and heat it to 70°C, add 10 g of sulfonating agent formaldehyde, heat it to 90°C, and keep it warm for 60 minutes;

[0027] (2) Cooling to 80°C, adding 10 g of liquid caustic soda and 8 g of maleic anhydride, heating to 95°C, and keeping warm for 10 minutes;

[0028] (3) Cooling to 40° C., adding 10 g of hydrogen peroxide, and spray drying to obtain a water-coal slurry additive with a solid content of 95%.

[0029] Example 2

[0030] A coal-water slurry additive using papermaking black liquor as raw material and a preparation method thereof, the specific steps are as follows:

[0031] (1) Add an aqueous solution of papermaking black liquor powder (100 g of papermaking black liquor powder and 300 g of deionized water) to the bottom of a kettle and heat it to 65° C., add 10 g of paraformaldehyde, heat it to 90° C., and keep it warm for 70 minutes;

[0032] (2) Cooling to 80°C, adding 8 g of hydrogen peroxide and 8 g of methyl methacrylate, heating to 95°C, and keeping warm for 10 minutes;

[0033] (3) Cooling to 40° C., adding 10 g of liquid alkali, and spray drying to obtain a water-coal slurry additive with a solid content of 95%.

[0034] Example 3

[0035] A coal-water slurry additive using papermaking black liquor as raw material and a preparation method thereof, the specific steps are as follows:

[0036] (1) Add 500 g of liquid papermaking black liquor (of which 100 g is dry weight) to the bottom of a kettle and heat it to 70° C., add 7 g of glyoxal, heat it to 80° C., and keep it warm for 70 minutes;

[0037] (2) Cooling to 70°C, adding 5 g of sodium persulfate, 4 g of liquid caustic soda, and 7 g of acrylonitrile, heating to 90°C, and keeping warm for 20 minutes;

[0038] (3) Cooling to 45° C., adding 5 g of sodium persulfate and 4 g of liquid caustic soda, and spray drying to obtain a water-coal slurry additive with a solid content of 95%.

[0039] Comparative Example 1

[0040] Sodium naphthalenesulfonate polymer (commercial coal water slurry additive).

[0041] Implementation Effect

[0042] Yanzhou coal and Yulin coal provided by Jining Mingsheng New Materials Co., Ltd. were used as raw materials, and samples of Examples 1-3 and Comparative Example 1 were added as additives to carry out water-coal slurry experiments. The performance of the obtained water-coal slurry was tested in accordance with the national standard GB / T18856.6-2002. The specific results are shown in Table 1-2.

[0043] Table 1 Yanzhou coal water slurry test results

[0044]

[0045]

[0046] Table 2 Yulin coal water slurry test results

[0047]

[0048] It can be seen from the above test results that when 0.18% of the water-coal slurry additive of the present invention is added to Yanzhou coal and Yulin coal, the product dosage is less, the pulping concentration is slightly better, the viscosity is slightly lower, the water separation rate and stability are slightly better than those of the control example, indicating that the water-coal slurry additive mixture prepared by modifying the papermaking black liquor can reduce costs and achieve the purpose of efficient utilization of biomass resources, and the water-coal slurry product produced has high concentration, low viscosity, good fluidity and good stability.

[0049] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of the present invention to be protected is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a water-coal slurry additive using papermaking black liquor as raw material, characterized in that: The specific steps are as follows: (1) heating 100 parts by weight of papermaking black liquor to 30-70° C., adding 10-20 parts by weight of one or more of formaldehyde, paraformaldehyde, and glyoxal, stirring evenly, and then continuing to heat to 70-100° C. and keeping the temperature for 30-120 minutes; (2) Cooling to 40-80°C, adding 5-10 parts by weight of a catalyst and 5-10 parts by weight of a cross-linking agent, heating to 80-110°C, and keeping warm for 10-90 minutes; (3) Cooling to 20-50° C., adding 5-10 parts by weight of a catalyst, and drying the feed liquid to obtain a water-coal slurry additive with a solid content of 85-100%; Wherein, the cross-linking agent is one or more of maleic anhydride, methyl methacrylate, and acrylonitrile; The catalyst is one or more of hydrogen peroxide, sodium persulfate, and liquid alkali.

2. The method for preparing a coal-water slurry additive using papermaking black liquor as raw material according to claim 1, characterized in that: The papermaking black liquor comprises an aqueous solution of papermaking black liquor dry powder or liquid papermaking black liquor; wherein, in the aqueous solution of the papermaking black liquor dry powder, the mass ratio of the papermaking black liquor dry powder to water is 1:2-4.

3. The method for preparing a water-coal slurry additive using papermaking black liquor as raw material according to claim 1, characterized in that: In the step (1), the temperature before adding one or more of formaldehyde, paraformaldehyde and glyoxal is 50-70° C., and the insulation time after adding one or more of formaldehyde, paraformaldehyde and glyoxal is 50-70 minutes.

4. The method for preparing a water-coal slurry additive using papermaking black liquor as raw material according to claim 1, characterized in that: In the step (2), the temperature before and after adding the catalyst and the cross-linking agent is 60-80°C and 85-105°C respectively, and the insulation time is 10-30 minutes.

5. The method for preparing a coal water slurry additive using papermaking black liquor as raw material according to claim 1, characterized in that: In the step (3), the temperature is lowered to 30-45°C; and the drying is performed by spray drying.