A method for measuring cross-sectional shrinkage of high-temperature tensile specimens

Through simulation experiments and sample immersion method, the area shrinkage of high-temperature tensile specimens is calculated, which solves the problem of measurement errors caused by irregular fracture shapes and improves the accuracy and safety of the continuous casting process.

CN116380685BActive Publication Date: 2024-10-22ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310293575.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-22
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

In the high-temperature tensile test, the irregular fracture shape of the sample makes it difficult to accurately measure the shrinkage rate, which affects the accuracy of the continuous casting process and the judgment of crack tendency.

Method used

A simulation experiment is used to obtain a rod-shaped cylindrical sample, which is heated, kept and stretched through a thermal simulation testing machine. It is broken into two sections and then butted into a whole. The relationship curve between the volume increment and the descending distance or time during the immersion of the sample into the solution is used. , calculate the shrinkage rate through curve slope analysis, avoiding measurement errors for irregular fracture shapes.

Benefits of technology

It achieves accurate measurement of the area shrinkage of high-temperature tensile specimens without being limited by the shape of the fracture, and improves the accuracy and safety of the continuous casting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116380685B_ABST
    Figure CN116380685B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for determining the mechanical properties of a metal material in a high-temperature tensile test, and in particular to a method for determining the cross-sectional shrinkage rate of a high-temperature tensile test specimen. The present invention establishes a relationship curve between the volume increment caused by the sample being immersed in a solution and the distance the sample falls or the time the sample falls at a uniform speed, finds the relationship between the cross-sectional area of ​​the sample before breaking or the cross-sectional area of ​​the sample at the fracture and the slope of the curve, and finally uses the slope of the curve at different positions to calculate the cross-sectional shrinkage rate of the sample after breaking. The method is not limited by the shape of the sample fracture, and can accurately determine the cross-sectional shrinkage rate of the sample even when the fracture is extremely irregular.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for measuring the mechanical properties of a metal material in a high-temperature tensile test, and in particular to a method for measuring the cross-sectional shrinkage of a high-temperature tensile test specimen. Background Art

[0002] At present, thermal simulation testing machines are widely used. According to the continuous casting process of the ingot, the sample is heated to the high temperature zone, kept in the high temperature zone for a period of time, then lowered to the set temperature, and finally stretched at a set stretching rate until the sample is broken. The cross-sectional area of ​​the sample after breaking is analyzed to obtain the cross-sectional shrinkage rate, which is used to study the plastic properties of the ingot during the continuous casting process.

[0003] The plasticity of the continuous casting billet is closely related to whether cracks occur in the billet after the continuous casting to bending and straightening process. Therefore, it is very important to accurately calculate the cross-sectional shrinkage rate of the fractured sample.

[0004] 201110081820.4 discloses a "clamping device for measuring the elongation and cross-sectional shrinkage of cylindrical tensile specimens". A set of devices is designed to center and fasten the specimens after they are pulled apart, and then a vernier caliper is used for relevant measurements. The problem solved by this patent document is to center and fasten the specimens for subsequent measurements, and it is mainly aimed at materials with regular cross-sections whose cross-sections after breaking are circular. CN200620045221.1 discloses a "quick measurement device for the elongation and cross-sectional shrinkage of circular specimens", and CN200820020540.6 discloses an "auxiliary clamping device for measuring the elongation and cross-sectional shrinkage of specimens". The same method of calculating cross-sectional shrinkage is used, and it is only applicable to regular cross-sections with circular fractures.

[0005] For fractures with regular cross-sectional shapes, such as circles or ellipses, the diameter or the length of the major and minor axes can be measured with a vernier caliper, and then the area can be calculated according to the area calculation formula for circles or ellipses; however, in the experimental process of simulating continuous casting, the sample undergoes necking under tensile stress under high temperature conditions. During the process of the sample necking and breaking, the surface of the sample flows in the direction of necking. For some materials, this fluidity is uneven, which can easily make the fracture shape obtained when the sample breaks irregular. The cross-sectional area of ​​the fracture cannot be calculated by simple measurement and using the area calculation formula. Therefore, it is impossible to accurately calculate the cross-sectional shrinkage rate of the sample at different temperatures, and it is difficult to make an accurate judgment on the tendency of continuous casting billets to crack.

[0006] Therefore, in view of the irregular cross-sectional shape of the specimen fracture, a better method is urgently needed to accurately measure the cross-sectional shrinkage rate of the high-temperature tensile specimen in order to guide the continuous casting process. Summary of the invention

[0007] In order to overcome the shortcomings of the prior art, the present invention provides a method for measuring the cross-sectional shrinkage of a high-temperature tensile specimen. The method is not limited by the shape of the specimen fracture and can accurately measure the cross-sectional shrinkage of the specimen even when the fracture is extremely irregular.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for measuring the cross-sectional shrinkage of a high-temperature tensile specimen, the method specifically comprising the following steps:

[0010] Step 1) obtaining a sample through a simulation experiment, wherein the simulation sample is a rod-shaped cylinder.

[0011] The simulated sample is heated, kept warm, cooled, and then stretched by a thermal simulation testing machine according to a predetermined experimental plan until the sample is broken to obtain a sample broken into two sections.

[0012] Step 2) The two sections of the sample are butt-joined to form a coaxial whole, and the two sections of the sample are joined by magnetization or adhesion to the state at the moment when the sample is stretched and broken.

[0013] Step 3) Take a container with sufficient solution and place it on a horizontal surface. The solution does not react with the sample. The axis of the two connected sample sections in step 2) is perpendicular to the liquid surface of the solution, and slowly placed in the solution along the direction perpendicular to the liquid surface of the solution.

[0014] During the insertion process, two methods are used: one is to descend the same distance d, mm each time; the other is to descend the sample at a constant speed, with a descending speed of v, mm / s. When descending, record the height of the solution level H, mm, and the total volume of the solution and the sample immersed in it V, ml.

[0015] Step 4) Draw a relationship curve between the total volume V, ml of the solution and the sample immersed therein and the sample falling distance d, mm, or the relationship curve between the total volume V, ml of the solution and the sample immersed therein and the sample falling time t, s in step 3).

[0016] When the sample is just immersed in the solution, the sample causes the liquid level to rise, causing the volume of the solution to increase. The increase is the volume of the part of the cylinder immersed in the solution. Since the cross-section of the cylinder is equal everywhere, the curve shows a straight rise.

[0017] When the terraced part of the sample is immersed in the solution, the cross section at this time gradually decreases as the sample descends, so the slope of the curve also decreases.

[0018] When the sample continues to descend to another section, the cross-section at this time gradually increases as the sample descends. Therefore, the slope of the curve also increases. Finally, the table-shaped part of the sample is completely immersed in the solution, and the increase in the solution volume is only affected by the volume of the cylinder immersed in the solution. The curve is in a straight upward state again.

[0019] Step 5) Based on the curve analysis drawn in step 4), the curve is differentiated in the first order to obtain the relationship curve between the slope K of the curve and the sample falling distance d, mm or the slope of the curve and the sample falling time t, s, where the slope K of the curve corresponds to the volume increment ΔV, ml.

[0020] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 . Based on the slope being proportional to the cross-sectional area, the following formula is obtained:

[0021] K 1 / S 1 =K 2 / S 2 (1)

[0022] Where: K 1 is the maximum slope of the curve;

[0023] S 1 is the maximum cross-sectional area of ​​the specimen, mm 2 ;

[0024] K 2 is the minimum slope of the curve;

[0025] S 2 is the minimum cross-sectional area of ​​the specimen at fracture, mm 2 ;

[0026] Step 6) Calculate the reduction of area.

[0027] The area of ​​the original cross-sectional circle of the specimen is S 1 , which is also the maximum value of the cross-sectional area of ​​the broken specimen. It is a known quantity. After the specimen is broken, the cross-sectional area at the fracture is the minimum cross-sectional area, which is S 2 , S can be obtained by formula (1) in step 5 2 Assume that the cross-sectional shrinkage rate is %, then we get:

[0028]

[0029] The S obtained by formula (1)2 Substituting into formula (2), we get the following formula:

[0030]

[0031] The cross-sectional shrinkage of the sample after high-temperature stretching can be obtained by formula (3).

[0032] Compared with the existing method, the beneficial effects of the present invention are:

[0033] For fractures with regular cross-sectional shapes, such as circles or ellipses, the diameter or the length of the major and minor axes can be measured with a vernier caliper, and then the area can be calculated using the area calculation formula for circles or ellipses. However, in the experimental process of simulated continuous casting, the fluidity is uneven, which can easily make the fracture shape obtained when the sample is broken irregular, and the cross-sectional area of ​​the fracture cannot be calculated by simple measurement using the area calculation formula.

[0034] The present invention establishes a relationship curve between the volume increment caused by the sample being immersed in a solution and the sample's descending distance or the sample's uniform descending time, finds the relationship between the cross-sectional area of ​​the sample before fracture or the cross-sectional area of ​​the sample at fracture and the slope of the curve, and finally uses the slope of the curve at different positions to calculate the cross-sectional shrinkage rate of the sample after fracture.

[0035] This method avoids the human errors in the measurement and calculation of cross-sectional area in the traditional calculation process of cross-sectional shrinkage rate, as well as the inability to measure and calculate the irregular cross-sectional area. This method is not limited by the fracture shape of the sample, and can accurately determine the cross-sectional shrinkage rate of the sample even when the fracture cross-sectional shape is extremely irregular. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the relationship between the total volume V of the solution of the present invention and the sample immersed therein and the distance d from which the sample descends;

[0037] Figure 2 It is a schematic diagram of the relationship between the total volume V of the solution of the present invention and the sample immersed therein and the sample falling time t;

[0038] Figure 3 Schematic diagram of the relationship between the total volume increment ΔV of the solution of the present invention and the sample immersed therein and the descending distance d of the sample;

[0039] Figure 4 It is a schematic diagram of a curve showing the relationship between the total volume increment ΔV of the solution of the present invention and the sample immersed therein and the sample falling time t;

[0040] Figure 5is a graph showing the relationship between the total volume V of the solution and the sample immersed therein and the descending distance d of the sample measured in Examples 1, 3 and 5 of the present invention;

[0041] Figure 6 is a graph showing the relationship between the total volume increment ΔV of the solution and the sample immersed therein and the descending distance d of the sample measured in Examples 1, 3 and 5 of the present invention;

[0042] Figure 7 is a graph showing the relationship between the total volume V of the solution and the sample immersed therein and the sample falling time t measured in Examples 2, 4 and 6 of the present invention;

[0043] Figure 8 It is a relationship curve between the total volume increment ΔV of the solution and the sample immersed therein and the sample falling time t measured in Examples 2, 4 and 6 of the present invention. DETAILED DESCRIPTION

[0044] The present invention discloses a method for determining the cross-sectional shrinkage rate of a high-temperature tensile specimen. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0045] A method for measuring the cross-sectional shrinkage of a high-temperature tensile specimen, the method specifically comprising the following steps:

[0046] Step 1) Obtain a sample through a simulation experiment. The simulation sample is a rod-shaped cylinder, and the simulation sample is heated, kept warm, and cooled according to a predetermined experimental plan using a thermal simulation test machine, and then stretched at 600 to 1400° C. until the sample is broken, thereby obtaining a sample broken into two sections.

[0047] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are butted together to form a whole, and the two sections are joined by magnetization or adhesion to the state of the sample at the moment of stretching and breaking.

[0048] Step 2) Take a container with sufficient solution and place it on a horizontal surface. The solution does not react with the sample. The axis of the two connected sample sections in step 2) is perpendicular to the liquid surface of the solution, and slowly placed in the solution along the direction perpendicular to the liquid surface of the solution.

[0049] During the insertion process, two methods can be used: one is to descend the same distance d, mm each time; the other is to descend the sample at a constant speed, with a descending speed of v, mm / s. When descending, record the height of the solution level H, mm, and the total volume of the solution and the sample immersed in it V, ml.

[0050] Step 3) Figure 1 , Figure 2 As shown, in step 2), a relationship curve is drawn between the total volume V, ml of the solution and the sample immersed therein and the distance d, mm the sample falls, or a relationship curve is drawn between the total volume V, ml of the solution and the sample immersed therein and the time t, s the sample falls.

[0051] When the sample is just immersed in the solution, the sample causes the liquid level to rise, causing the volume of the solution to increase. The increase is the volume of the part of the cylinder immersed in the solution. Since the cross-section of the cylinder is equal everywhere, the curve shows a straight rise.

[0052] When the terraced part of the sample is immersed in the solution, the cross section at this time gradually decreases as the sample descends, so the slope of the curve also decreases.

[0053] When the sample continues to descend to another section, the cross-section at this time gradually increases as the sample descends. Therefore, the slope of the curve also increases. Finally, the table-shaped part of the sample is completely immersed in the solution, and the increase in the solution volume is only affected by the volume of the cylinder immersed in the solution. The curve is in a straight upward state again.

[0054] Step 4) Figure 3 , Figure 4 As shown, based on the curve analysis drawn in step 3), the curve is differentiated in the first order to obtain the relationship curve between the slope K of the curve and the sample falling distance d, mm or the slope K of the curve and the sample falling time t, s. The slope K of the curve corresponds to the volume increment ΔV, ml.

[0055] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 . Based on the slope being proportional to the cross-sectional area, the following formula is obtained:

[0056] K 1 / S 1 =K 2 / S 2 (1)

[0057] Where: K 1 is the maximum slope of the curve;

[0058] S 1 is the maximum cross-sectional area of ​​the specimen, mm 2 ;

[0059] K 2 is the minimum slope of the curve;

[0060] S 2 is the minimum cross-sectional area of ​​the specimen at fracture, mm 2 ;

[0061] Step 5) Calculate the cross-sectional shrinkage.

[0062] The area of ​​the original cross-sectional circle of the specimen is S 1 , which is also the maximum value of the cross-sectional area of ​​the broken specimen. It is a known quantity. After the specimen is broken, the cross-sectional area at the fracture is the minimum cross-sectional area, which is S 2 , S can be obtained by formula (1) in step 4 2 Assume that the cross-sectional shrinkage rate is %, then we get:

[0063]

[0064] The S obtained by formula (1) 2 Substituting into formula (2), we get the following formula:

[0065]

[0066] The cross-sectional shrinkage of the sample after high-temperature stretching can be obtained by formula (3).

[0067] The present invention measures the cross-sectional shrinkage rate of a high-temperature tensile specimen after fracture by a specimen drainage method, which is not only applicable to fractures of regular shapes, but also breaks through the measurement of cross-sectional shrinkage rates of fractures of irregular shapes. The relationship curve between the volume increment caused by the specimen immersion in the solution and the specimen descent distance or the uniform descent time is used to find the relationship between the cross-sectional area of ​​the specimen before fracture or the cross-sectional area of ​​the specimen fracture and the slope of the curve, and finally the cross-sectional shrinkage rate of the specimen after fracture is calculated by using the slope of the curve at different positions. The method is not limited by the shape of the specimen fracture, and can accurately measure the cross-sectional shrinkage rate of the specimen even when the fracture is extremely irregular.

[0068] [Example]

[0069] Embodiment 1:

[0070] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ by a thermal simulation test machine, kept warm for 5 minutes, then cooled to 1000℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 1×10 -3 s -1 , until the sample is broken to obtain a sample broken into two pieces.

[0071] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0072] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample that have been connected in step 1 perpendicular to the water surface and slowly place them in the solution. During the placement process, lower them by the same distance of 0.5 mm each time.

[0073] 3. Draw the relationship curve between the total volume of water and the part of the sample immersed in water and the distance the sample falls in step 2, such as Figure 5 shown.

[0074] 4. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the distance d of the sample, as shown in Figure 6 shown.

[0075] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 72.35% using formulas (1), (2) and (3).

[0076] Embodiment 2:

[0077] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ through a thermal simulation test machine, kept warm for 5 minutes, and then cooled to 1000℃ at a rate of 3℃ / s. Then it is kept warm for 1 minute and stretched. The stretching rate is set to 1×10- 3 s -1 , until the sample is broken to obtain a sample broken into two pieces.

[0078] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0079] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample connected in step 1 perpendicular to the water surface and slowly place it in the solution. During the placement process, the sample descends at a constant speed, and the descending speed is v = 1mm / s;

[0080] 3. Draw a curve showing the relationship between the total volume of water and the part of the sample immersed in water and the time it takes for the sample to fall in step 2, such as Figure 7 As shown;

[0081] 4. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the sample drop time t, such as Figure 8 shown.

[0082] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 71.34% using formulas (1), (2) and (3).

[0083] Embodiment 3:

[0084] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ through a thermal simulation test machine, kept warm for 5 minutes, then cooled to 700℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 1×10 -3 s -1 , until the sample is broken to obtain a sample broken into two pieces.

[0085] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0086] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample that have been connected in step 1 perpendicular to the water surface and slowly place them in the solution. During the placement process, lower them by the same distance of 0.5 mm each time.

[0087] 3. Draw the relationship curve between the total volume of water and the part of the sample immersed in water and the distance the sample falls in step 2, such as Figure 5 shown.

[0088] 4. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the distance d of the sample, as shown in Figure 6 Show.

[0089] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 35.27% using formulas (1), (2) and (3).

[0090] Embodiment 4:

[0091] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ through a thermal simulation test machine, kept warm for 5 minutes, then cooled to 700℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 1×10 -3 s -1 , until the sample is broken to obtain a sample broken into two pieces.

[0092] Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0093] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample connected in step 1 perpendicular to the water surface and slowly place it in the solution. During the placement process, the sample descends at a constant speed, and the descending speed is v = 1mm / s;

[0094] 3. Draw a curve showing the relationship between the total volume of water and the part of the sample immersed in water and the time it takes for the sample to fall in step 2, such as Figure 7 shown.

[0095] 3. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the sample drop time t, such as Figure 8 shown.

[0096] 4. Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 35.69% using formulas (1), (2) and (3).

[0097] Embodiment 5:

[0098] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ through a thermal simulation test machine, kept warm for 5 minutes, then cooled to 1200℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 1×10 -3 s -1 , until the sample is broken, and a sample is obtained that is broken into two sections. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0099] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample that have been connected in step 1 perpendicular to the water surface and slowly place them in the solution. During the placement process, lower them by the same distance of 0.5 mm each time.

[0100] 3. Draw the relationship curve between the total volume of water and the part of the sample immersed in water and the distance the sample falls in step 2, such as Figure 5 shown.

[0101] 4. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the distance d of the sample, as shown in Figure 7 shown.

[0102] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 61.97% using formulas (1), (2) and (3).

[0103] Embodiment 6:

[0104] 1. Obtain the sample through simulation experiment. The material selected is a kind of low carbon steel, and it is processed into a simulation sample with a size of Φ10×125mm cylinder. It is heated to 1300℃ through a thermal simulation test machine, kept warm for 5 minutes, then cooled to 1200℃ at a rate of 3℃ / s, and then kept warm for 1 minute for stretching. The stretching rate is set to 1×10 -3 s -1 , until the sample is broken, and a sample is obtained that is broken into two sections. Based on the deformation behavior of the sample at high temperature, the sample is broken into two sections, one end of each section near the fracture is in a table shape, and the rest is in a cylindrical shape. The two sections of the sample are magnetized and butted together to form a whole.

[0105] 2. Take a container filled with sufficient water and place it on a horizontal surface. Place the axis of the two sections of the sample connected in step 1 perpendicular to the water surface and slowly place it in the solution. During the placement process, the sample descends at a constant speed, and the descending speed is v = 1mm / s;

[0106] 3. Draw a curve showing the relationship between the total volume of water and the part of the sample immersed in water and the time it takes for the sample to fall in step 2, such as Figure 7 shown.

[0107] 4. Based on the curve analysis drawn in step 3, the curve is differentiated in the first order to obtain the relationship curve between the slope of the curve and the sample drop time t, such as Figure 8 shown.

[0108] Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 Since the slope is proportional to the cross-sectional area, the cross-sectional shrinkage of the sample can be determined to be 62.05% using formulas (1), (2) and (3).

[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for determining the cross-sectional shrinkage of a high-temperature tensile specimen. It is characterized in that The method specifically comprises the following steps: Step 1) selecting a rod-shaped sample; heating, keeping warm, cooling the sample, and then stretching the sample until the sample is broken to obtain a sample broken into two sections; Step 2) butting the two sections of the sample together so that they are coaxial and become a whole, and joining the two sections of the sample to the state at the moment when the sample is stretched and broken; Step 3) placing the container on a horizontal surface, and injecting a solution that does not react with the sample into the container; The axis of the sample after docking in step 2) is perpendicular to the liquid surface of the solution, and the sample is placed in the solution along the direction perpendicular to the liquid surface of the solution; During the insertion process, two methods are used: one is to descend the same distance d, mm each time; the other is to descend the sample at a uniform speed, with a descending speed of v, mm / s; When descending, record the height of the solution surface H, mm, and the total volume of the solution and the sample immersed therein V, ml; Step 4) drawing a relationship curve between the total volume V, ml, of the solution and the sample immersed therein and the distance d, mm, of the sample falling, or the relationship curve between the total volume V, ml, of the solution and the portion of the sample immersed in the solution and the time t, s, of the sample falling in step 3); Step 5) Performing first-order differentiation on the curve of step 4) to obtain a curve showing the relationship between the slope K of the curve and the sample descending distance d, mm or the slope K of the curve and the sample descending time t, s, wherein the slope K of the curve corresponds to the volume increment ΔV, ml; Maximum slope of the curve K 1 Corresponding to the maximum cross-sectional area of ​​the sample S 1 , the minimum slope of the curve K 2 Corresponding to the minimum cross-sectional area of ​​the specimen S 2 The minimum cross-sectional area at the fracture of the specimen is S 2 ; Based on the slope being proportional to the cross-sectional area, the following formula is obtained: K 1 / S 1 =K 2 / S 2 (1) Where: K 1 is the maximum slope of the curve; S 1 is the maximum cross-sectional area of ​​the specimen, mm 2 ; K 2 is the minimum slope of the curve; S 2 is the minimum cross-sectional area of ​​the specimen at fracture, mm 2 ; Step 6) calculating the section shrinkage; The area of ​​the original cross-sectional circle of the specimen is S 1 , which is also the maximum value of the cross-sectional area of ​​the broken specimen. It is a known quantity. After the specimen is broken, the cross-sectional area at the fracture is the minimum cross-sectional area, which is S 2 , and obtain S by formula (1) in step 5 2 , assuming the cross-sectional shrinkage rate is %, then we get: The S obtained by formula (1) 2 Substituting into formula (2), we get the following formula: The cross-sectional shrinkage of the sample after high-temperature stretching is obtained by formula (3).

2. A method for measuring cross-sectional shrinkage of a high-temperature tensile specimen according to claim 1, It is characterized in that In the step 1), a rod-shaped cylindrical sample is selected.

3. A method for measuring cross-sectional shrinkage of a high-temperature tensile specimen according to claim 1, It is characterized in that In the step 1), the simulated sample is heated, kept warm, cooled, and then stretched by a thermal simulation test machine according to a predetermined experimental plan until the sample is broken to obtain a sample broken into two sections.

4. A method for measuring cross-sectional shrinkage of a high-temperature tensile specimen according to claim 1, It is characterized in that In the step 2), the two sections of the sample are joined together by magnetization or adhesion to form a state at the moment when the sample is stretched and broken.

5. The method for measuring the cross-sectional shrinkage of a high-temperature tensile specimen according to claim 1, It is characterized in that In the step 4), when the sample is just immersed in the solution, the curve rises in a straight line; when the table-shaped part of the sample is immersed in the solution, the slope of the curve decreases; when the sample continues to descend to another section, the slope of the curve increases; finally, when the table-shaped part of the sample is completely immersed in the solution, the curve rises in a straight line again.