A method for preparing high carbonization active cementitious material by desulfurization of phosphogypsum

Through scientific proportioning and temperature control processes, we can efficiently desulfurize phosphogypsum and prepare highly carbonized active cementitious materials, which solves the application limitations and environmental pollution problems of phosphogypsum in the preparation of cement clinker, and realizes high-efficiency, low-energy phosphorus gypsum production. Utilization of gypsum resources.

CN116395994BActive Publication Date: 2024-10-29HUAXIN CEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310321112.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-29
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The desulfurization rate of phosphogypsum is difficult to reach above 95%, which limits the application of phosphogypsum in cement clinker preparation, and the existing process has problems of high energy consumption and environmental pollution.

Method used

Using low-cost conventional raw materials, the phosphogypsum, carbonaceous raw materials and silicon-aluminum-iron raw materials are dried, crushed and ground to form pellets, which are desulfurized, and then calcareous raw materials are added to adjust the KH value and then enter the rotary kiln for calcination. , scientific proportioning and temperature control to prepare highly carbonized active gelling materials.

Benefits of technology

The high-efficiency desulfurization rate of phosphogypsum has reached more than 99%, and a highly carbonized active cementitious material based on γ-C2S has been prepared. It has the characteristics of environmental friendliness, low energy consumption and short carbonization time, and the self-pulverizing material does not require powder. Grinding increases strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116395994B_ABST
    Figure CN116395994B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum, wherein phosphogypsum is mixed and ground with carbonaceous raw materials and ferro-silicon raw materials according to the molar ratio of C in the carbonaceous raw materials to SO3 in the phosphogypsum of 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6, water is added to form a material ball, and then dried; the dried material ball is placed in a desulfurization furnace for desulfurization of CaSO4; after the obtained desulfurized material is cooled, a calcium raw material is added to adjust the KH value, and then mixed and ground, and finally enters a rotary kiln for calcination, and a high carbonization active cementitious material is obtained after natural cooling. The present invention adopts low-priced conventional raw materials, can process phosphogypsum in large quantities, enables phosphogypsum to obtain a better desulfurization effect, and prepares an environmentally friendly, low-energy-consuming, γ-C2S mineral-based, carbon-absorbing, and short carbonization time High carbonization active cementitious material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for preparing a high-carbonization active cementitious material by desulfurizing phosphogypsum. Background Art

[0002] Phosphogypsum is a solid waste produced in the wet phosphoric acid process. The composition of phosphogypsum is relatively complex. In addition to hydrated calcium sulfate, there are also incompletely decomposed phosphate ore, residual phosphoric acid, fluoride, acid insoluble matter, organic matter, etc. Among them, the presence of fluorine and organic matter has the greatest impact on the resource utilization of phosphogypsum. Stacking will occupy a large amount of land and cause pollution to water and land resources. At present, there is no better way to utilize phosphogypsum. Its resource utilization and safe and efficient utilization are of great significance to solving the environmental pollution and resource waste problems caused by stacking treatment.

[0003] In 1969, the Austrian Linz Company completed and put into operation a plant for producing cement from phosphogypsum and sulfuric acid. In the 1980s, my country also built 7 sets of equipment. The main method is to dry and dehydrate the phosphogypsum, mix it with coke, clay, sandstone, etc. according to the clinker ratio, and calcine it in a hollow rotary kiln to produce clinker. The SO2 in the kiln gas is converted and absorbed to produce sulfuric acid. However, the strength of cement produced from phosphogypsum is generally low, and it even fails to reach the strength grade of 42.5 ordinary Portland cement. At present, most of the co-production units have been shut down.

[0004] Compared with CaCO3, CaSO4 needs a higher temperature to be completely decomposed and desulfurized, which will increase the difficulty and cost of the process operation. It can still exist in large quantities even at the temperature of clinker calcination, which undoubtedly restricts its application in cement clinker preparation. There are many literature reports on the decomposition of phosphogypsum using carbonaceous raw materials, carbon monoxide atmosphere, elemental sulfur, etc., but it is difficult to achieve a desulfurization rate of more than 95% for phosphogypsum by the reduction of carbon and sulfur alone. If the desulfurization rate does not meet this requirement, it will have many adverse effects on the production and application of clinker.

[0005] In addition to using phosphogypsum as a CaO source to replace natural limestone and thus reduce limestone usage and carbon emissions, using the excellent CO2 absorption capacity, high carbonization activity and self-pulverization properties of γ-C2S (gamma-type dicalcium silicate) minerals to prepare high-performance materials and thus reduce carbon emissions has also been a hot research topic in recent years.

[0006] How to process phosphogypsum in large quantities to achieve better desulfurization effect of phosphogypsum and prepare environmentally friendly, low-energy consumption, high-carbonization active cementitious materials mainly composed of γ-C2S minerals, with strong carbon absorption capacity and short carbonization time has become a technical problem that needs to be solved urgently. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a high-carbonization active cementitious material by desulfurizing phosphogypsum, which adopts low-cost conventional raw materials, can process a large amount of phosphogypsum, so that the phosphogypsum can obtain a better desulfurization effect, and prepare an environmentally friendly, low-energy-consuming, high-carbonization active cementitious material mainly composed of γ-C2S minerals, with strong carbon absorption capacity and short carbonization time.

[0008] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0009] A method for preparing a high carbonization active cementitious material by desulfurizing phosphogypsum comprises the following steps:

[0010] (1) obtaining phosphogypsum, carbonaceous raw materials, and silicon-aluminum-iron raw materials, drying, crushing, mixing, and grinding after mixing;

[0011] (2) adding water to the obtained mixture to form pellets, and then drying;

[0012] (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4;

[0013] (4) After the desulfurized material is cooled, calcium raw materials are added to adjust the KH value, and then mixed and ground, and finally sent to a rotary kiln for calcination. After natural cooling, a high carbonization active cementitious material is obtained.

[0014] According to the above scheme, the carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.

[0015] According to the above scheme, the ferro-aluminum-silicon raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, and fly ash.

[0016] According to the above scheme, the scientific ingredients described in step (1) are that the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6.

[0017] According to the above scheme, the diameter of the ball in step (2) is 1-3 cm.

[0018] According to the above scheme, the desulfurization temperature of the desulfurization furnace in step (3) is 1150-1250°C.

[0019] According to the above scheme, the calcium raw material in step (4) is one or more raw materials mainly containing CaO, such as limestone, quicklime, slaked lime, etc.

[0020] According to the above scheme, the KH value in step (4) is 0.6-0.7.

[0021] According to the above scheme, the calcination temperature of the rotary kiln in step (4) is 1200-1300°C.

[0022] According to the above scheme, the mineral composition of the high carbonization active cementitious material obtained in step (4) is mainly γ-C2S, wherein the content of γ-C2S is ≥70%.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The invention can process a large amount of phosphogypsum, and the percentage of CaO provided by the phosphogypsum in the obtained high-carbonization active cementitious material accounts for more than 65% of the total CaO content.

[0025] A large amount of phosphogypsum can be used to produce a high carbonization active cementitious material with a γ-C2S content of ≥70%. It can be self-pulverized without the need for grinding, and the carbonization time required to achieve a higher strength is short.

[0026] Making the material into balls can reduce the contact between the carbonaceous raw materials in the balls and the air, making it easier to create a reducing atmosphere, thereby reducing the waste of carbonaceous raw materials.

[0027] On the premise that low KH value allows SiO2 to promote CaSO4 desulfurization to form a more stable and easier to generate mineral C2S, a lower KH value and total CaO:SiO2 are used to provide more SiO2 for desulfurization and lower the eutectic temperature, thereby solving the problem that the sphere is more difficult to burn and desulfurize than powder due to uneven heating and atmosphere conditions.

[0028] The raw materials used are all low-priced conventional raw materials in cement clinker production and can be obtained locally. After scientific formulation, the desulfurization effect of phosphogypsum is good and stable, the desulfurization rate reaches more than 99%, and the SO3 content in the calcined product is ≤1%. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : XRD spectrum of the high carbonization activity gelling material obtained in Example 1. DETAILED DESCRIPTION

[0030] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0031] A specific embodiment provides a method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum:

[0032] (1) obtaining phosphogypsum, carbonaceous raw materials, and silicon-aluminum-iron raw materials, drying, crushing, scientifically proportioning, and then mixing and grinding;

[0033] (2) adding water to the obtained mixture to form pellets, and then drying;

[0034] (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4;

[0035] (4) After the desulfurized material is cooled, calcium raw materials are added to adjust the KH value, and then mixed and ground, and finally sent to a rotary kiln for calcination. After natural cooling, a high carbonization active cementitious material is obtained.

[0036] Specifically, the carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.

[0037] Specifically, the ferro-aluminum raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, fly ash, and various types of waste residues.

[0038] Specifically, the scientific ingredients in step (1) are as follows: the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6.

[0039] Specifically, the diameter of the ball in step (2) is 1-3 cm.

[0040] Specifically, the desulfurization temperature of the desulfurization furnace in step (3) is 1150-1250°C.

[0041] Specifically, the calcium raw material in step (4) is one or more of raw materials mainly containing CaO, such as limestone, quicklime, slaked lime, etc.

[0042] Specifically, the KH value in step (4) is 0.6-0.7.

[0043] Specifically, the calcination temperature of the rotary kiln in step (4) is 1200-1300°C.

[0044] Specifically, the mineral composition of the high carbonization activity cementitious material obtained in step (4) is mainly γ-C2S, wherein the content of γ-C2S is ≥70%.

[0045] The acquisition and detection of raw materials in the following specific examples:

[0046] Obtain phosphogypsum and silicon-aluminum-iron raw materials, and perform chemical composition analysis after drying, crushing and grinding. For example, the chemical composition of a batch of phosphogypsum, coal gangue and limestone obtained randomly is shown in Table 1:

[0047] Table 1 Chemical composition analysis

[0048] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 limestone 39.84 5.66 1.29 1.02 48.33 2.64 0.05 0.29 0.15

[0049] The carbonaceous raw material used was subjected to conventional analysis and chemical composition analysis of the ash, which is high-sulfur coal. The results are shown in Table 2 and Table 3 respectively:

[0050] Table 2 Conventional analysis of high sulfur coal

[0051] name Moisture Ash Volatile Matter Fixed carbon content Total sulfur Qnet,ad Qnet,d High sulfur coal 1.42 23.48 10.25 64.85 2.99 25.25 26.33

[0052] Table 3 Chemical composition analysis of high sulfur coal ash

[0053] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40

[0054] Example 1

[0055] 1. Ratio design of phosphogypsum desulfurization

[0056] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss of 19.27% ​​+ 42.46% = 61.73%. The remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.475, the SM value is 6.629, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.491. The design ratio is that the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal is 86: 14: 6.88, and the weight of ash introduced by high-sulfur coal is 6.88 * 0.2348 = 1.62. The ratio and corresponding indicators are shown in Table 4 and Table 5 respectively:

[0057] Table 4 Proportions

[0058] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 14 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62

[0059] Table 5 Indicators corresponding to the ratio

[0060]

[0061] 2. Ball making

[0062] The phosphogypsum, coal gangue and high-sulfur coal measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.

[0063] 3. Desulfurization of phosphogypsum

[0064] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1200°C.

[0065] 4. Add calcium raw materials and calcine to obtain high carbonization active cementitious materials

[0066] Add calcium raw materials to the desulfurized materials for mixed grinding. The calcium raw materials used here are limestone, and the amount of limestone is equivalent to 20 in the desulfurization ingredients, so that the KH value is 0.623. The proportions of high carbonization active cementitious materials and the corresponding indicators are shown in Table 6 and Table 7 respectively:

[0067] Table 6 Proportion

[0068] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 14 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62 limestone 39.84 5.66 1.29 1.02 48.33 2.64 0.05 0.29 0.15 20

[0069] Table 7 Indicators corresponding to the ratio

[0070]

[0071] Then it enters the rotary kiln for calcination, and after natural cooling, a high carbonization active gelling material is obtained. The temperature of the rotary kiln is set at 1250°C.

[0072] 5. Carbonization

[0073] The self-pulverized high carbonization active cementitious material was made into cylindrical specimens with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa and a water-solid ratio of 0.15. They were carbonized for 2 h and 24 h respectively under the conditions of a carbon dioxide concentration of 100%, a temperature of 25°C, a humidity of 60%, and an air pressure of 0.3 MPa, and then the compressive strength was measured.

[0074] Example 2

[0075] 1. Ratio design of phosphogypsum desulfurization

[0076] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss of 19.27% ​​+ 42.46% = 61.73%. The remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.449, the SM value is 6.699, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.417. The design ratio is that the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal is 85:15:6.8, and the weight of ash introduced by high-sulfur coal is 6.8 * 0.2348 = 1.60. The ratio and corresponding indicators are shown in Table 8 and Table 9 respectively:

[0077] Table 8 Proportions

[0078] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 85 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 15 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.60

[0079] Table 9 Indicators corresponding to the ratio

[0080]

[0081] 2. Ball making

[0082] The phosphogypsum, coal gangue and high-sulfur coal measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.

[0083] 3. Desulfurization of phosphogypsum

[0084] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1180°C.

[0085] 4. Add calcium raw materials and calcine to obtain high carbonization active cementitious materials

[0086] Add calcium raw materials to the desulfurized materials for mixed grinding. The calcium raw materials used here are limestone. The amount of limestone is equivalent to 22 in the desulfurization ingredients, making the KH value 0.607. The proportions of high carbonization active cementitious materials and the corresponding indicators are shown in Table 10 and Table 11 respectively:

[0087] Table 10 Proportions

[0088] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 85 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 15 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.60 limestone 39.84 5.66 1.29 1.02 48.33 2.64 0.05 0.29 0.15 22

[0089] Table 11 Indicators corresponding to the ratio

[0090]

[0091] Then it enters the rotary kiln for calcination, and after natural cooling, a high carbonization active gelling material is obtained. The temperature of the rotary kiln is set at 1240°C.

[0092] 5. Carbonization

[0093] The self-pulverized high carbonization active cementitious material was made into cylindrical specimens with a diameter of 2 cm and a height of 2 cm at a molding pressure of 10 MPa and a water-solid ratio of 0.15. They were carbonized for 2 h and 24 h respectively under the conditions of a carbon dioxide concentration of 100%, a temperature of 25°C, a humidity of 60%, and an air pressure of 0.3 MPa, and then the compressive strength was measured.

[0094] Comparative Example 1

[0095] 1. Ratio design of phosphogypsum desulfurization

[0096] Directly adopt the ratio of step 4 of Example 1 for desulfurization, calculate the SO3 in the chemical composition of phosphogypsum into its own ignition loss, according to the ignition loss 19.27% ​​+ 42.46% = 61.73%, the remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.623, and the SM value is 6.00. 2. The mass ratio of total CaO to SiO2 in the chemical composition is 1.923 for design proportion, that is, the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal: limestone is 86: 14: 6.88, the weight of ash introduced by high-sulfur coal is 6.88 * 0.2348 = 1.62, the proportion and corresponding indicators are shown in Table 12 and Table 13 respectively:

[0097] Table 12 Proportions

[0098] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 14 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62 limestone 39.84 5.66 1.29 1.02 48.33 2.64 0.05 0.29 0.15 20

[0099] Table 13 Indicators corresponding to the ratio

[0100]

[0101] 2. Ball making

[0102] The phosphogypsum, coal gangue, high-sulfur coal and limestone measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.

[0103] 3. Desulfurization of phosphogypsum

[0104] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1200°C.

[0105] In addition to the temperature of 1150-1250° C. described in the present invention, each embodiment and comparative example further added 1100° C. during the desulfurization of phosphogypsum. The content of SO3 in the desulfurized material is shown in Table 14, and the SO3 content is measured by total sulfur analysis.

[0106] Table 14 SO3 content in desulfurized materials

[0107]

[0108] According to the research of our institute, when the KH is 0.6-0.7, the total CaO:SiO2 is 1.8-2.3:

[0109] (1) Formation of aluminum-iron phase mineral C in the ingredients 12The part of CaSO4 in A7, C3A, C4AF and C2F relies on Fe2O3 and Al2O3 for desulfurization. The desulfurization effect of Fe2O3 and Al2O3 on CaSO4 is worse than that of SiO2.

[0110] (2) Al2O3 combines with CaO and CaSO4 to form by-product minerals, which inhibit further desulfurization;

[0111] (3) C4AF and C2F are also difficult to burn in a reducing atmosphere and cannot be formed well, resulting in a decrease in the direct desulfurization effect of Fe2O3 on CaSO4 (the part of CaSO4 required to form iron-phase minerals) and the indirect desulfurization effect (fluxing to promote the formation of C2S);

[0112] (4) The desulfurization of CaSO4 has reached the limit chemical equilibrium that can be adjusted under the KH at this time, and the SO3 content is between 1% and 3%. After using conventional raw materials, the SO3 content in the calcined product is 2%.

[0113] The present invention, under the condition of carbonaceous raw materials providing a reducing atmosphere, is based on a method in which SiO2 promotes the desulfurization of CaSO4 to form a more stable and easier-to-generate mineral C2S based on low KH (KH value is 0.6-0.7) ingredients, and continues to optimize and improve the method, reducing KH to a total CaO:SiO2 ratio of less than 2, providing more SiO2 for desulfurization, so that all CaSO4 has SiO2 and excess SiO2 is matched to generate calcium silicate-containing minerals, allowing the desulfurization chemical balance of SiO2 on CaSO4 to continue to move in the direction of desulfurization, and reducing the negative impact of Fe2O3 and Al2O3 that cannot further desulfurize CaSO4.

[0114] Compared with Example 1, Comparative Example 1 directly adopts the ratio of step 4 in Example 1 for desulfurization, mainly because the KH value of phosphogypsum during desulfurization is higher (total CaO:SiO2 is higher), that is, the company has made a breakthrough in the decomposition and desulfurization of phosphogypsum in recent research, and applied for an invention patent for "a process for desulfurization and co-production of cement of phosphogypsum", which mainly adopts a method of mixing and desulfurization with low KH value ingredients, with a KH value of 0.6-0.7, so that SiO2 promotes the desulfurization of CaSO4 to form a more stable and easier to generate mineral C2S, but the SO3 content after calcination at 1100°C is 1-3%, which cannot be reduced to below 1%, and the desulfurization is carried out in powder form. In Comparative Example 1, the pellets are subjected to uneven heating and atmosphere conditions compared to the powdery state, making them difficult to burn and desulfurize. In addition, when KH is 0.66, the high SM value aggravates the difficulty in burning due to insufficient liquid phase minerals. Therefore, the SO3 content reaches 10.13% after calcination at 1100°C; the difficulty in burning is improved after the temperature reaches 1200°C, and the final SO3 content is 2-3%.

[0115] In Example 1 and Example 2, based on the premise that SiO2 promotes CaSO4 desulfurization at low KH value to form a more stable and easier to generate mineral C2S, a lower KH value and total CaO:SiO2 are used to provide more SiO2 for desulfurization and reduce the eutectic temperature, thereby solving the problem that the sphere is difficult to burn and desulfurize due to uneven heating and atmosphere conditions compared to powder at high SM value. The higher SM value reduces the negative impact of Fe2O3 and Al2O3 in not being able to further desulfurize CaSO4, and successfully reduces the final SO3 content to less than 1%. A high desulfurization rate has been achieved at 1100℃, and desulfurization is based on the formation of C2S.

[0116] The KH value and the total CaO to SiO2 mass ratio during desulfurization in Example 2 are slightly lower than those in Example 1, which makes the melting point lower. In addition, a large amount of CaSO4 itself has a strong fluxing effect during the desulfurization process, resulting in slight melting of the sample. If the KH value continues to decrease to below 0.4, it will be unfavorable for production due to severe melting, and the desulfurization effect of CaSO4 will also deteriorate.

[0117] The main mineral contents in the prepared high carbonization activity cementitious material are shown in Table 15, and the carbonization conditions and the strength after carbonization are shown in Table 16.

[0118] Table 15 Main mineral contents in the prepared high carbonization activity cementitious materials

[0119] project Calcination temperature <![CDATA[γ-C2S]]> <![CDATA[β-C2S]]> <![CDATA[SiO2]]> <![CDATA[Ca2Al2SiO7]]> <![CDATA[CaSO4]]> Example 1 1250℃ 77.4 16.5 0.8 4.0 0.4 Example 2 1240℃ 76.6 17.3 1.0 3.3 0.8

[0120] Table 16 Carbonization conditions and strength after carbonization of high carbonization activity cementitious materials

[0121]

[0122] The high carbonization active cementitious materials obtained in Example 1 and Example 2 both achieved self-pulverization under natural cooling conditions, did not require grinding, and had good carbonization performance, reaching a high strength after carbonization for 2 hours. Figure 1 This is the XRD spectrum of the high carbonization active cementitious material prepared in Example 1. The jade quantitative analysis results are γ-C2S=77.4%, β-C2S=16.5%, and the content of γ-C2S, a high carbonization active mineral, is high.

[0123] Table 17 Percentage of CaO in each raw material to the total CaO content

[0124]

[0125] The percentage of CaO in each raw material to the total CaO content is shown in Table 17. The percentage of CaO provided by phosphogypsum to the total CaO content is above 65%. The amount of phosphogypsum used in the ingredients of the present invention is large, and the CaO in the prepared high carbonization active cementitious material is mainly provided by phosphogypsum.

[0126] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum, characterized in that The following steps are involved: (1) obtaining phosphogypsum, carbonaceous raw materials, and ferrosilicon-aluminum raw materials, drying, crushing, mixing and grinding the raw materials; the mixing materials are such that the molar ratio of C in the carbonaceous raw materials to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6; (2) Add water to the obtained mixture to form pellets, and then dry them; (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4; the desulfurization temperature of the desulfurization furnace is 1150-1250°C; (4) After the desulfurized material is cooled, calcium raw materials are added to adjust the KH value to 0.6-0.7, and then mixed and ground. Finally, the mixture is calcined in a rotary kiln. After natural cooling, a high carbonization active cementitious material is obtained. The calcination temperature of the rotary kiln is 1200-1300°C.

2. The method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.

3. The method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The ferro-aluminum-silicon raw material in step (1) is one or more of sandstone, coal gangue, silica, clay and fly ash.

4. The method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The diameter of the ball in step (2) is 1-3 cm.

5. The method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The calcium raw material in step (4) is one or more of limestone, quicklime and slaked lime.

6. The method for preparing a high carbonization active cementitious material by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The mineral composition of the high carbonization active cementitious material obtained in step (4) is mainly γ-C2S, wherein the content of γ-C2S is ≥70%.

Citation Information

Patent Citations

  • Method for preparing low-calcium self-pulverization clinker and co-producing sulfuric acid by utilizing phosphogypsum

    CN114644466A

  • Process for co-production of cement by desulfurization of phosphogypsum

    CN115073030A