A retarder for concrete and preparation method thereof
The retarder is prepared through a combination of bentonite and other raw materials in a specific proportion, which solves the problems of excessive air entrainment and low hydration degree of concrete in the existing technology, significantly prolongs the setting time of concrete, improves fluidity and compactness, and ensures Construction performance.
Patent Information
- Application Number
- CN202310320346.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing concrete retarders lead to excessive air entrainment of concrete and low hydration, making it difficult to ensure the initial and final setting time standards of concrete and affecting performance.
Using a combination of bentonite, high molecular organic polymers, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride, calcium formate, methyl cyanate, epoxy resin, polyaluminum ferric chloride and polyaluminum silicate sulfate, etc. The retarder is prepared through stirring reaction and freeze-drying, and the pH value and ratio are adjusted to form a stable compound to extend the setting time of concrete.
It significantly extends the setting time of concrete, improves fluidity and compactness, reduces the shrinkage and crack incidence of concrete, and ensures ideal performance and strength during construction.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to a retarder for concrete and a preparation method thereof. Background Art
[0002] Retarder is an admixture that can delay the cement hydration reaction, thereby extending the setting time of concrete, making the newly mixed concrete maintain plasticity for a longer time, facilitating pouring, and improving construction efficiency. At the same time, it will not cause adverse effects on the various properties of concrete in the later stage. There are many types of retarders, which can be divided into two categories according to their chemical composition: inorganic retarders and organic retarders. Among them, inorganic retarders include: phosphates, zinc salts, iron sulfate, copper sulfate, borates, fluorosilicates, etc.; organic retarders include: lignin sulfonates, hydroxycarboxylic acids and their salts, polyols and their derivatives, sugars and carbohydrates, etc. At present, concrete retarders will cause excessive air entrainment in concrete, resulting in low hydration degree and small hydration products, which will affect the later strength. It is difficult to ensure the performance of concrete while meeting the initial and final setting time standards. Summary of the invention
[0003] In view of this, the present invention provides a retarder for concrete and a preparation method thereof to solve the above problems.
[0004] The technical solution of the present invention is achieved as follows: a retarder for concrete comprises the following raw materials in parts by weight: 5-12 parts of bentonite, 1-3 parts of high molecular organic polymer, 0.3-0.9 parts of borax, 1-6 parts of hydroxyethylidene diphosphonic acid, 2-6 parts of cyclic acid anhydride, 1.3-2.5 parts of calcium formate, 0.2-0.8 parts of methyl cyanate, 0.1-0.3 parts of epoxy resin, 0.3-0.5 parts of polyaluminium chloride ferric, 0.1-0.4 parts of polyaluminium silicate sulfate and 45-88 parts of water.
[0005] Furthermore, a retarder for concrete includes the following raw materials in parts by weight: 8 parts of bentonite, 2 parts of polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminum ferric chloride, 0.3 parts of polyaluminum silicate sulfate, and 62 parts of water.
[0006] Furthermore, the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 3.2-8.9:1.3-2.8:0.6-1.0.
[0007] Furthermore, the cyclic anhydride is any one of phthalic anhydride, maleic anhydride or succinic anhydride.
[0008] Furthermore, the epoxy resin is one or a combination of bisphenol A epoxy resin or novolac epoxy resin.
[0009] Furthermore, the epoxy resin is a bisphenol A epoxy resin and a novolac epoxy resin in a weight ratio of 1:1-3.
[0010] Furthermore, the water is deionized water or distilled water.
[0011] Furthermore, the method for preparing a retarder for concrete comprises the following steps:
[0012] S1. After ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 70-80° C. for 12-24 hours to obtain a mixture I;
[0013] S2, taking methyl cyanate, bisphenol A epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing at a speed of 400-600 rpm to obtain a mixture II;
[0014] S3, mixing the above-mentioned mixed material I and mixed material II, stirring and mixing at a temperature of 60-80° C. to obtain mixed material III;
[0015] S4. After the mixture III is cooled, it is filtered and washed 2-4 times, the pH is adjusted to 7.35-7.45, and then freeze-dried at -30 to -50°C for 20-40 hours to obtain a concrete retarder.
[0016] Furthermore, the stirring rate in S1 is 400-600 rpm.
[0017] Furthermore, the stirring and dispersion of S2 is performed for 18-25 minutes.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The retarder of the invention has obvious retarding effect, significantly prolongs the setting time of cement paste, and achieves a strong retarding effect. The retarder prepared by scientifically matching the raw materials has a certain retarding effect. Increasing the proportion of bentonite and borax is helpful to disperse cement particles, reduce the surface tension of concrete, improve the flowability of concrete, and prolong the plastic deformation time of concrete. The polymer can maintain the flowability of concrete at a specific proportion and prevent the temperature inside the concrete from rising, thereby achieving a better retarding effect. Polyaluminium ferric chloride and polyaluminium silicate sulfate can react with calcium ions in water and silicate ions in concrete to form a stable compound, thereby slowing down the hardening speed of concrete.
[0020] The retarder of the present invention can be applied to concrete to prolong the setting time of concrete, thereby allowing the concrete to maintain fluidity for a long time during the construction process, making it convenient for workers to adjust and handle, reducing the temperature of concrete, and preventing problems such as cracking and deformation caused by excessively high concrete temperature. The setting time of concrete can be accurately controlled, thereby ensuring that the concrete achieves ideal performance and strength during the construction process, improving the fluidity of concrete, thereby improving the uniformity and density of concrete, reducing the shrinkage of concrete, and reducing the incidence of concrete cracks. DETAILED DESCRIPTION
[0021] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0022] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0023] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0024] Example 1
[0025] A retarder for concrete: the following raw materials are weighed in parts by weight: 5 parts of bentonite, 1 part of high molecular organic polymer, 0.3 parts of borax, 1 part of hydroxyethylidene diphosphonic acid, 2 parts of cyclic acid anhydride, 1.3 parts of calcium formate, 0.2 parts of methyl cyanate, 0.1 parts of epoxy resin, 0.3 parts of polyaluminium ferric chloride, 0.1 parts of polyaluminium silicate sulfate, and 45 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 3.2:1.3:0.6; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:1; the water is deionized water;
[0026] The retarder was prepared according to the following method:
[0027] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 75° C. and 500 rpm for 18 h to obtain a mixture I;
[0028] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 500 rpm for 22 minutes to obtain a mixture II;
[0029] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 70° C. for 5 minutes to obtain mixture III;
[0030] S4: After the mixture III is cooled, it is filtered and washed twice, the pH is adjusted to 7.35, and then freeze-dried at -30°C for 20 hours to obtain a concrete retarder.
[0031] Example 2
[0032] A retarder for concrete: the following raw materials are weighed in parts by weight: 12 parts of bentonite, 3 parts of high molecular organic polymer, 0.9 parts of borax, 6 parts of hydroxyethylidene diphosphonic acid, 6 parts of cyclic acid anhydride, 2.5 parts of calcium formate, 0.8 parts of methyl cyanate, 0.3 parts of epoxy resin, 0.5 parts of polyaluminium ferric chloride, 0.4 parts of polyaluminium silicate sulfate, and 88 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 8.9:2.8:1.0; the cyclic acid anhydride is maleic anhydride; the epoxy resin is bisphenol A epoxy resin and novolac epoxy resin in a weight ratio of 1:3; the water is distilled water;
[0033] The retarder is prepared according to the following method:
[0034] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 75° C. and 500 rpm for 18 h to obtain a mixture I;
[0035] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 500 rpm for 22 minutes to obtain a mixture II;
[0036] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 70° C. for 5 min to obtain mixture III;
[0037] S4. After the mixture III is cooled, it is filtered and washed 4 times, the pH is adjusted to 7.45, and then freeze-dried at -50°C for 40 hours to obtain a concrete retarder.
[0038] Example 3
[0039] A retarder for concrete: the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminium ferric chloride, 0.3 parts of polyaluminium silicate sulfate and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone and polyoxyethylene ether in a weight ratio of 5.2:2.5:0.8; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:2; and the water is deionized water.
[0040] The retarder was prepared according to the following method:
[0041] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 75° C. and 500 rpm for 18 h to obtain a mixture I;
[0042] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 500 rpm for 22 minutes to obtain a mixture II;
[0043] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 70° C. for 5 min to obtain mixture III;
[0044] S4. After the mixture III is cooled, it is filtered and washed twice, the pH is adjusted to 7.35, and then freeze-dried at -30°C for 20 hours to obtain a concrete retarder.
[0045] Example 4
[0046] A retarder for concrete: the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminium ferric chloride, 0.3 parts of polyaluminium silicate sulfate, and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 5.2:2.5:0.8; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:2; the water is deionized water;
[0047] The retarder was prepared according to the following method:
[0048] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 70° C. and 400 rpm for 12 h to obtain a mixture I;
[0049] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 400 rpm for 18 minutes to obtain a mixture II;
[0050] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 60° C. for 5 minutes to obtain mixture III;
[0051] S4. After the mixture III is cooled, it is filtered and washed three times, the pH is adjusted to 7.4, and then freeze-dried at -40°C for 30 hours to obtain a concrete retarder.
[0052] Example 5
[0053] A retarder for concrete: the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminium ferric chloride, 0.3 parts of polyaluminium silicate sulfate, and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 5.2:2.5:0.8; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:2; the water is deionized water;
[0054] The retarder was prepared according to the following method:
[0055] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 80° C. and 600 rpm for 24 h to obtain a mixture I;
[0056] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 600 rpm for 25 minutes to obtain a mixture II;
[0057] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 80° C. for 5 minutes to obtain mixture III;
[0058] S4. After the mixture III is cooled, it is filtered and washed three times, the pH is adjusted to 7.4, and then freeze-dried at -40°C for 30 hours to obtain a concrete retarder.
[0059] Comparative Example 1
[0060] The difference between this comparative example and Example 3 is that the retarder weighs the following raw materials in parts by weight: 2 parts of bentonite, 5 parts of high molecular organic polymer, 0.1 parts of borax, 8 parts of hydroxyethylidene diphosphonic acid, 8 parts of cyclic acid anhydride, 3.8 parts of calcium formate, 0.1 parts of methyl cyanate, 0.5 parts of epoxy resin, 0.2 parts of polyaluminium chloride ferric, 0.7 parts of polyaluminium silicate sulfate, and 35 parts of water;
[0061] The retarder is prepared according to the following method:
[0062] S1, after ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 75° C. and 500 rpm for 18 h to obtain a mixture I;
[0063] S2, taking methyl cyanate, epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and dispersing them at a speed of 500 rpm for 22 minutes to obtain a mixture II;
[0064] S3, mixing the above-mentioned mixture I and mixture II, stirring and mixing at a temperature of 70° C. for 5 minutes to obtain mixture III;
[0065] S4. After the mixture III is cooled, it is filtered and washed three times, the pH is adjusted to 7.4, and then freeze-dried at -40°C for 30 hours to obtain a concrete retarder.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 3 is that the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 2:1:0.3. Specifically, the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminum chloride ferric, 0.3 parts of polyaluminum silicate sulfate, and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 2:1:0.3; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and novolac epoxy resin in a weight ratio of 1:2; and the water is deionized water.
[0068] Comparative Example 3
[0069] The difference between this comparative example and Example 3 is that the raw material of the retarder does not contain polyaluminium chloride ferric. Specifically, the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.3 parts of polyaluminium silicate sulfate, and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 5.2:2.5:0.8; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:2; and the water is deionized water.
[0070] Comparative Example 4
[0071] The difference between this comparative example and Example 3 is that the raw material of the retarder does not contain polyaluminium silicate sulfate. Specifically, the following raw materials are weighed in parts by weight: 8 parts of bentonite, 2 parts of high molecular organic polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminium chloride ferric, and 62 parts of water; the high molecular organic polymer is polyacrylamide, polyvinyl pyrrolidone, and polyoxyethylene ether in a weight ratio of 5.2:2.5:0.8; the cyclic acid anhydride is phthalic anhydride; the epoxy resin is bisphenol A epoxy resin and phenolic epoxy resin in a weight ratio of 1:2; and the water is deionized water.
[0072] 1. Performance test:
[0073] The retarders prepared in the above Examples 1-5 and Comparative Examples 1-4 and commercially available retarders were added to concrete materials at an amount of 0.2wt%, and the prepared concrete products were tested for slump, expansion, initial setting time, final setting time and compressive strength. The slump test standard is GB / T50080-2016; the expansion test standard is GB / T 50080-2016; the compressive strength test standard is GB / T 50107-2010; the initial setting time is measured from the time when water is added until the time when the concrete loses its plasticity; the final setting time is the time required for the cement slurry to completely lose its plasticity and begin to generate strength after the cement is mixed with water.
[0074] The test results are shown in the following table:
[0075] Slump / mm Expansion / mm Initial setting time / h Final setting time / h 28-day compressive strength / MPa Example 1 195 511 62 69 85.1 Example 2 196 508 60 68 84.4 Example 3 195 510 63 71 86.9 Example 4 201 509 61 63 84.7 Example 5 203 503 58 60 83.6 Comparative Example 1 209 495 51 53 70.9 Comparative Example 2 204 493 49 51 71.2 Comparative Example 3 201 487 42 49 68.9 Comparative Example 4 199 489 41 45 66.8 Commercially available 226 479 8.6 9.9 62.7
[0076] Result analysis: The retarder of the present invention has a retarding effect that is significantly better than that of commercially available retarders, and significantly prolongs the setting time of cement paste, indicating that the retarder prepared by the present invention effectively inhibits the splash of cement and achieves a strong retarding effect; Example 3 is compared with Comparative Example 1, indicating that the retarder prepared under a suitable formula has a certain retarding effect, and increasing the ratio of bentonite and borax is helpful to disperse cement particles, reduce the surface tension of concrete, improve the flowability of concrete, and prolong the plastic deformation time of concrete; compared with Comparative Example 2, the polymer can maintain the fluidity of concrete at a specific ratio and prevent the temperature inside the concrete from rising, thereby achieving a better retarding effect; compared with Comparative Examples 3 and 4, polyaluminum ferric chloride and polyaluminum silicate sulfate can react with calcium ions in water and silicate ions in concrete to form a stable compound, thereby slowing down the hardening speed of concrete.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A retarder for concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 5-12 parts of bentonite, 1-3 parts of polymer, 0.3-0.9 parts of borax, 1-6 parts of hydroxyethylidene diphosphonic acid, 2-6 parts of cyclic acid anhydride, 1.3-2.5 parts of calcium formate, 0.2-0.8 parts of methyl cyanate, 0.1-0.3 parts of epoxy resin, 0.3-0.5 parts of polyaluminium ferric chloride, 0.1-0.4 parts of polyaluminium silicate sulfate and 45-88 parts of water; the polymer comprises polyacrylamide, polyvinyl pyrrolidone and polyoxyethylene ether in a weight ratio of 3.2-8.9:1.3-2.8:0.6-1.
0.
2. The retarder for concrete according to claim 1, characterized in that: The method comprises the following raw materials in parts by weight: 8 parts of bentonite, 2 parts of polymer, 0.6 parts of borax, 3 parts of hydroxyethylidene diphosphonic acid, 4 parts of cyclic acid anhydride, 1.9 parts of calcium formate, 0.6 parts of methyl cyanate, 0.2 parts of epoxy resin, 0.4 parts of polyaluminium ferric chloride, 0.3 parts of polyaluminium silicate sulfate and 62 parts of water.
3. The retarder for concrete according to claim 1, characterized in that: The cyclic anhydride is any one of phthalic anhydride, maleic anhydride or succinic anhydride.
4. The retarder for concrete according to claim 1, characterized in that: The epoxy resin is one or a combination of bisphenol A epoxy resin or novolac epoxy resin.
5. The retarder for concrete according to claim 4, characterized in that: The epoxy resin is a bisphenol A epoxy resin and a novolac epoxy resin in a weight ratio of 1:1-3.
6. The retarder for concrete according to claim 1, characterized in that: The water is deionized water.
7. The method for preparing a retarder for concrete according to claim 1, characterized in that: The following steps are involved: S1. After ball-milling bentonite, polymer, borax, hydroxyethylidene diphosphonic acid, cyclic acid anhydride and calcium formate, water was added, and the mixture was stirred at 70-80° C. for 12-24 hours to obtain a mixture I; S2, taking methyl cyanate, bisphenol A epoxy resin, polyaluminium chloride ferric, and polyaluminium silicate sulfate, mixing and dispersing them evenly, stirring and mixing at a speed of 400-600 rpm to obtain a mixture II; S3, mixing the above-mentioned mixed material I and mixed material II, stirring and mixing at a temperature of 60-80° C. to obtain mixed material III; S4. After the mixture III is cooled, it is filtered and washed 2-4 times, the pH is adjusted to 7.35-7.45, and then freeze-dried at -30 to -50°C for 20-40 hours to obtain a concrete retarder.
8. The method for preparing a retarder for concrete according to claim 7, characterized in that: The stirring rate in S1 is 400-600 rpm.
9. The method for preparing a retarder for concrete according to claim 7, characterized in that: The stirring and mixing time of S2 is 18-25 minutes.