A method for extracting germanium from germanium-containing lignite
By using ammonia water for leaching treatment and acid precipitation treatment, germanium is extracted from germanium-containing lignite, which solves the problems of high-concentration hydrochloric acid consumption and environmental pollution in the existing technology, and achieves efficient, environmentally friendly germanium extraction and comprehensive utilization of resources.
Patent Information
- Application Number
- CN202211489491.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-25
AI Technical Summary
Existing methods for extracting germanium from lignite have problems such as high consumption of high-concentration hydrochloric acid, large production of waste acid, difficulty in harmless disposal of residues, and low comprehensive utilization of resources, resulting in environmental pollution and unsatisfactory economic benefits.
Using ammonia water as the leaching agent, germanium is extracted from germanium-containing lignite through leaching treatment, including leaching treatment, solid-liquid separation, and acid precipitation treatment, to obtain a germanium-containing solution, and use residual coal and humic acid substances as organic fertilizers.
It significantly improves the leaching rate of germanium, realizes a green and environmentally friendly extraction process, reduces chemical consumption and environmental hazards, and synergistically separates organic matter and germanium, improving the comprehensive utilization rate of resources.
Smart Images

Figure CN116397114B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to germanium extraction technology, in particular to a method for extracting germanium from germanium-containing lignite. Background Art
[0002] As a strategic resource, germanium is increasingly widely used in modern industries, such as semiconductors, fiber-optic communications, infrared optics, solar cells, chemical and light industries, food industries, germanium alloys and many other fields. Lignite is a type of low-rank coal with abundant reserves in my country. As an important source of scattered metallic germanium, germanium is "naturally present" in lignite. Combining with organic matter is the main state of occurrence of germanium in coal. Due to the development of side chains and functional groups of lignite molecules, it has more organic complexing sites, so almost all germanium-rich coals with industrial value belong to lignite. Germanium-rich lignite is one of the strategic metal minerals, in which germanium is abnormally enriched, usually with a germanium content of more than 20μg / g, and has a high comprehensive utilization value.
[0003] At present, the main method in industry is to enrich the germanium-containing raw materials into germanium concentrate and then extract them by chlorination distillation. The extraction of germanium from fly ash after lignite combustion by chlorination distillation has been industrially applied for more than 50 years. The technology is relatively mature, the equipment complexity is low, and the germanium recovery rate is generally around 60%. However, as the first step in the extraction process, the leaching step requires the use of high-concentration hydrochloric acid to achieve selective dissolution and strengthen the dissolution process. There are technical and cost problems such as strong system acidity, large hydrochloric acid consumption, large amount of waste acid generated, and difficult harmless disposal of residues. In addition, lignite has a low combustion calorific value and produces large pollution, which is not conducive to the ecological environment. Although there are leaching methods such as organic acid leaching and water leaching to leach germanium from fly ash, the economic benefits are not ideal due to cost and technical problems.
[0004] In summary, the existing leaching method of germanium in germanium coal mines is mainly chlorination leaching. During the combustion of lignite, the organic matter in lignite cannot be efficiently utilized, the comprehensive utilization rate of resources is low, and the waste acid and waste residue produced are harmful to the environment. Summary of the invention
[0005] To overcome at least one of the defects of the above-mentioned prior art, in a first aspect, an embodiment of the present invention provides a method for extracting germanium from germanium-containing lignite, comprising extracting germanium from the germanium-containing lignite by leaching treatment using ammonia water as a leaching agent.
[0006] According to one embodiment of the present invention, the method comprises the following steps:
[0007] S1: providing a first mixture, wherein the first mixture comprises germanium-containing lignite and ammonia water;
[0008] S2: subjecting the first mixture to leaching treatment to obtain a second mixture; and
[0009] S3: performing solid-liquid separation on the second mixture, and then performing acid precipitation treatment on the separated liquid to obtain a third mixture; and
[0010] S4: performing solid-liquid separation on the third mixture to obtain a germanium-containing solution.
[0011] According to one embodiment of the present invention, the temperature of the leaching treatment is 80-280°C.
[0012] According to one embodiment of the present invention, the leaching treatment time is 3 to 4 hours.
[0013] According to one embodiment of the present invention, the pressure of the leaching treatment is 0.5-0.9 MPa.
[0014] According to one embodiment of the present invention, the leaching treatment is performed under nitrogen protection, and the pressure of the nitrogen is 0.5-0.9 MPa.
[0015] According to one embodiment of the present invention, step S3 comprises: performing solid-liquid separation on the second mixture to obtain residual coal and a solution containing humic acid substances, adjusting the pH value of the solution containing humic acid substances to 1 to 1.5 for the acid precipitation treatment, and the solution containing humic acid substances contains humate.
[0016] According to one embodiment of the present invention, in the step S3 or S4, the solid-liquid separation is performed by suction filtration or centrifugation.
[0017] According to one embodiment of the present invention, the residual coal is used as organic fertilizer.
[0018] According to one embodiment of the present invention, the step S4 comprises: subjecting the third mixture to solid-liquid separation and drying treatment to obtain humic acid substances and a germanium-containing solution.
[0019] According to one embodiment of the present invention, the humic acid substances are used as organic fertilizers.
[0020] In a method for extracting germanium from germanium-containing lignite according to an embodiment of the present invention, the leaching rate of germanium is significantly improved, and the method is green and environmentally friendly, and the organic matter of the obtained coal can be modified and effectively recovered.
[0021] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.
[0023] in:
[0024] Figure 1 The present invention is a process flow chart of extracting germanium from germanium-containing lignite according to one embodiment of the present invention. DETAILED DESCRIPTION
[0025] The preferred embodiments of the present invention are described in detail below, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0026] An embodiment of the present invention provides a method for extracting germanium from germanium-containing lignite, comprising extracting germanium from the germanium-containing lignite through a leaching process using ammonia water as a leaching agent.
[0027] A method for extracting germanium from germanium-containing lignite according to an embodiment of the present invention comprises the following steps:
[0028] S1: providing a first mixture, the first mixture comprising germanium-containing lignite and ammonia water;
[0029] S2: subjecting the first mixture to a leaching treatment to obtain a second mixture; and
[0030] S3: performing solid-liquid separation on the second mixture, and then performing acid precipitation treatment on the separated liquid to obtain a third mixture; and
[0031] S4: performing solid-liquid separation on the third mixture to obtain a germanium-containing solution.
[0032] In one embodiment, residual coal, humic acid substances and germanium-containing solution can be obtained by processing the second mixture and the third mixture; wherein the residual coal and humic acid substances are rich in nitrogen and can be used as modified nitrogen-rich organic fertilizers.
[0033] A method for extracting germanium from germanium-containing lignite according to one embodiment of the present invention is a technology for mildly precipitating germanium through ammoniation. The method has a high germanium leaching rate and can achieve the coordinated separation of organic matter and scattered metallic germanium. The leaching process conditions are mild, and compared with the existing methods, the consumption of reagents is reduced, and the harm of the leaching process to the environment is reduced. Other products can be used as nitrogen-rich organic fertilizers instead of being burned, thereby reducing the waste of resources caused by the burning process.
[0034] In one embodiment, the germanium-containing lignite may be germanium-rich lignite, and the germanium content thereof is above 20 μg / g.
[0035] The present invention does not limit the amount of ammonia water used. Preferably, an excess amount of ammonia water is used so that all substances that can participate in the reaction in the germanium-containing lignite can react.
[0036] In one embodiment, in step S1, the ground germanium-containing lignite and the leaching agent ammonia water can be uniformly mixed in a certain proportion, wherein the mass of the ammonia water can be 10 to 20 times the mass of the germanium-containing lignite, for example, 12 times, 14 times, 15 times, 16 times, or 18 times.
[0037] In one embodiment, the mass percentage concentration of the raw ammonia water in step S1 can be 5-20%, for example, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%.
[0038] In one embodiment, the temperature of the leaching treatment can be 80-280°C, for example, 100°C, 120°C, 140°C, 150°C, 160°C, 180°C, 200°C, 220°C, 240°C, 250°C, 260°C.
[0039] In one embodiment, the leaching treatment time may be 3 to 4 hours, for example 3.5 hours.
[0040] In one embodiment, the pressure of the leaching treatment may be 0.5-0.9 MPa, such as 0.6 MPa, 0.7 MPa, or 0.8 MPa.
[0041] In one embodiment, the stirring rate of the first mixture during the leaching process can be 700-800 r / min, for example, 710 r / min, 720 r / min, 740 r / min, 750 r / min, 760 r / min, 780 r / min.
[0042] In one embodiment, nitrogen may be used as the protective gas for the leaching process, and the pressure of the nitrogen may be 0.5-0.9 MPa, such as 0.6 MPa, 0.7 MPa, or 0.8 MPa.
[0043] In one embodiment, in step S2, a micro autoclave can be used as a container for leaching treatment. Further, the first mixture can be placed in a micro autoclave, nitrogen gas of a certain pressure can be introduced as a protective gas, heating and stirring can be turned on, the temperature can be raised to a set temperature, and the leaching treatment can be started.
[0044] In one embodiment, after the temperature in the micro-autoclave drops to 20-28° C. (eg, 22° C., 24° C., 25° C., 26° C.), the second mixture obtained by the leaching treatment is taken out from the autoclave.
[0045] In one embodiment, in step S3, the second mixture can be subjected to solid-liquid separation by suction filtration or centrifugation to obtain solid and liquid; further, the solid-liquid separation operation can be repeated 3 to 5 times, for example 4 times.
[0046] In one embodiment, in step S3, the separated solid is washed with water and dried to obtain nitrogen-rich residual coal. The number of washing times can be 3 to 6 times, for example, 4 times or 5 times. The separated liquid and the solution obtained after washing the solid are both nitrogen-rich solutions containing humic acid substances. The washed solution can be mixed with the liquid obtained by solid-liquid separation.
[0047] In one embodiment, the solution containing humic acid substances includes humic acid substances, and the humic acid substances include humic acid and / or humate salts; further, the solution containing humic acid substances includes humate salts, such as black humate salts, brown humate salts and yellow humate salts.
[0048] In one embodiment, in step S3, acid is added to the solution containing humic acid substances for acid precipitation, so that the humate therein is converted into humic acid; further, the solution containing humic acid substances is acidified by adding acid to adjust the pH to 1-1.5, and the pH can be, for example, 1.1, 1.2, 1.3, or 1.4.
[0049] In one embodiment, in step S4, the third mixture obtained by acid precipitation is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute germanium-containing solution. The nitrogen-rich humic acid substances include humic acid, which includes but is not limited to black humic acid and brown humic acid; the dilute germanium-containing solution is a low-salt germanium solution containing trace soluble organic matter. Subsequently, the dilute germanium-containing solution can be deeply enriched by solvent extraction or ion exchange to obtain a germanium-rich solution with a simpler composition and a higher germanium content, and the germanium can be precipitated by tannin precipitation for recovery.
[0050] The raw material for extracting germanium in the existing chlorination distillation technology is fly ash produced after coal combustion, which has a low leaching rate, a large amount of waste acid, a germanium recovery rate of generally 60%, and the combustion process pollutes the environment. The method for extracting germanium from germanium-containing lignite according to one embodiment of the present invention uses ammonia water as a leaching agent for ammonia leaching, and the germanium leaching rate can reach more than 90%, and further more than 95%; compared with traditional chlorination leaching, the reagent pH is weaker, the conditions are relatively mild, the germanium leaching rate is significantly improved, and a large amount of waste acid will not be generated, reducing the harm of the leaching process to the environment. The product can be used as a nitrogen-rich organic fertilizer, reducing the waste of resources and environmental pollution caused by the combustion process.
[0051] According to a method for extracting germanium from germanium-containing lignite in one embodiment of the present invention, after leaching operation, the yield of the obtained coal is above 80%, and it can be effectively recovered without destroying the basic organic structure in the coal. The residual coal and humic acid substances can be used as modified nitrogen-rich organic fertilizers.
[0052] The method for extracting germanium from germanium-containing lignite according to one embodiment of the present invention has a short process flow, high comprehensive resource utilization rate, and low environmental pollution, thereby realizing high-value and clean utilization of lignite, saving costs, and having significant economic benefits. Moreover, the main micro-high-pressure reactor equipment used is mature and easy to industrialize.
[0053] The method for extracting germanium from germanium-containing lignite according to one embodiment of the present invention can directly and efficiently and gently leach germanium from the germanium-rich lignite, and can realize the comprehensive utilization of lignite organic matter.
[0054] Hereinafter, a method for extracting germanium from germanium-containing lignite according to an embodiment of the present invention will be further described in conjunction with the accompanying drawings and specific examples.
[0055] The calculation formula for germanium leaching rate is:
[0056] m 残煤 Indicates the mass of residual coal, a 残煤 Indicates the germanium content in residual coal, m 原煤 Indicates the quality of raw coal, a 残煤 Indicates the germanium content in raw coal. Raw coal refers to the raw material containing germanium lignite.
[0057] Example 1
[0058] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0059] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 80° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0060] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0061] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 90.68%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 92.96%.
[0062] Example 2
[0063] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0064] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 120° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0065] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0066] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 98.73%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 90.18%.
[0067] Example 3
[0068] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0069] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 160° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0070] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0071] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 97.89%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 87.44%.
[0072] Example 4
[0073] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0074] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 200° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0075] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0076] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 98.96%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 88.74%.
[0077] Example 5
[0078] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0079] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 240° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0080] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0081] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 98.82%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 81.24%.
[0082] Example 6
[0083] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 15% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0084] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 280° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0085] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0086] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 97.65%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 83.46%.
[0087] Example 7
[0088] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 5% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0089] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 200° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0090] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the total solution is adjusted to pH 1-1.5 and acid precipitation is performed to obtain a third mixture.
[0091] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 95.11%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 86.52%.
[0092] Example 8
[0093] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 10% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0094] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 200° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0095] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0096] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 96.03%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 86.33%.
[0097] Example 9
[0098] S1: Weigh 5 g of germanium-rich lignite (germanium content 128 g / t) that has passed a 200 sieve, and mix it evenly with 20% ammonia water to obtain a first mixture; wherein the amount of ammonia water added is 10 times the weight of the germanium-rich lignite.
[0099] S2: placing the first mixture in a micro high-pressure reactor, introducing nitrogen as a protective gas, the pressure of the nitrogen being 0.5 MPa; starting heating and stirring, raising the temperature to 200° C. for leaching treatment, and the leaching time being 3 hours; during this process, germanium is leached into the solution.
[0100] S3: After the leaching is completed, the mixture in the kettle is taken out, and solid-liquid separation is repeated three times by suction filtration; the separated solid is washed with deionized water five times, and nitrogen-rich residual coal is obtained after drying, and weighed; the separated solution is a nitrogen-rich solution containing humic acid substances, and the above washing solution is added to the separated solution; the pH of the obtained solution is adjusted to 1-1.5, and the third mixture is obtained by acid precipitation.
[0101] S4: The third mixture is subjected to solid-liquid separation and then dried to obtain nitrogen-rich humic acid substances and a dilute solution containing germanium, and the humic acid substances are weighed; wherein germanium enters the dilute solution containing germanium in the form of germanic acid, and the germanium content is determined by ICP-OES after digestion, and the germanium leaching rate is calculated according to formula (1) to be 97.48%; the sum of the masses of the nitrogen-rich residual coal and the nitrogen-rich humic acid substances is the mass of the recovered coal, and the coal yield is 88.97%.
[0102] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for extracting germanium from germanium-containing lignite, comprising extracting germanium from the germanium-containing lignite by leaching using ammonia water as a leaching agent, comprising the following steps: S1: providing a first mixture, wherein the first mixture comprises germanium-containing lignite and ammonia water; S2: subjecting the first mixture to leaching treatment to obtain a second mixture; and S3: performing solid-liquid separation on the second mixture, and then performing acid precipitation treatment on the separated liquid to obtain a third mixture; and S4: performing solid-liquid separation on the third mixture to obtain a germanium-containing solution.
2. The method according to claim 1, wherein: The leaching treatment temperature is 80 to 280° C.; and / or, The leaching treatment time is 3 to 4 hours.
3. The method according to claim 1, wherein: The pressure of the leaching treatment is 0.5-0.9 MPa.
4. The method according to claim 1, wherein: The leaching treatment is carried out under nitrogen protection, and the pressure of the nitrogen is 0.5-0.9 MPa.
5. The method according to claim 1, wherein: The step S3 comprises: The second mixture is subjected to solid-liquid separation to obtain residual coal and a solution containing humic acid substances, and the pH value of the solution containing humic acid substances is adjusted to 1-1.5 for the acid precipitation treatment.
6. The method according to claim 5, wherein: The step S4 comprises: performing solid-liquid separation and drying treatment on the third mixture to obtain humic acid substances and a germanium-containing solution.
7. The method according to claim 6, wherein: The residual coal or the humic acid substance is used as an organic fertilizer.
8. The method according to claim 6, wherein: The humic acid substances include humic acid and / or humate.
9. The method according to claim 1, wherein: In the step S3 or S4, the solid-liquid separation is performed by suction filtration or centrifugation.
Citation Information
Patent Citations
Method for Germanium Humic Acid
KR1020140126486A