Controllable synthesis and preparation method of a type of bismuth-based oxysulfide one-dimensional material

The VLS method is used to grow Bi2O2Te/Bi2TeO5 one-dimensional materials on thermally evaporated gold silicon wafers or drop-coated gold silicon wafers, which solves the problem of zero synthesis of Bi2O2Te and Bi2TeO5 one-dimensional materials, achieves controllable preparation of materials, and fills the research gap. It also demonstrates the characteristics of easy operation, high safety and strong controllability.

CN116443822BActive Publication Date: 2024-10-15SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310377814.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-15
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

There are currently no reports on the synthesis and research of Bi2O2Te and Bi2TeO5 one-dimensional materials. The lack of effective preparation methods limits their application in the field of micro-nano electronics.

Method used

The VLS method is used to grow Bi2O2Te/Bi2TeO5 one-dimensional materials on thermally evaporated gold silicon wafers or drop-coated gold silicon wafers. By heating Bi2Te3 powder with high-purity argon gas or argon oxygen in a dual-temperature zone tube furnace, the reaction conditions are controlled to To achieve material growth.

Benefits of technology

Bi2O2Te/Bi2TeO5 one-dimensional materials were successfully prepared with simple process, low temperature and strong controllability, filling the gap in zero synthesis of Bi2O2Te/Bi2TeO5 one-dimensional materials. It has the advantages of easy operation, high safety and strong controllability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116443822B_ABST
    Figure CN116443822B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of semiconductor / dielectric material technology, and specifically relates to a controllable synthesis preparation method of a type of bismuth-based oxygen-sulfur one-dimensional material. The method is specifically as follows: first weigh a certain mass of Bi2Te3 powder as a precursor and place it in a high temperature zone, and use a thermally evaporated gold silicon wafer or a drop-coated gold silicon wafer as a substrate and place it in a low temperature zone, and after vacuuming, the temperature of the two temperature zones is increased to the target temperature at a certain rate, and then a carrier gas is introduced to grow the one-dimensional material, and after the growth is completed, the carrier gas is stopped, and it is naturally cooled to room temperature, and the Bi2O2Te / Bi2TeO5 one-dimensional material is prepared. The method of the present invention has the advantages of simple operation, high safety, strong controllability, etc., and fills the blank of zero synthesis of Bi2O2Te / Bi2TeO5 one-dimensional materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor / dielectric materials, and in particular relates to a controllable synthesis preparation method of a bismuth-based oxysulfide one-dimensional material. Background Art

[0002] Two-dimensional layered materials play a vital role in many fields such as electronic devices, optoelectronics and energy conversion, and information storage because of their ultra-thin atomic layer thickness, high specific surface area, good flexibility, and tunable band structure, and they exhibit quantum effects that are completely different from those of traditional materials. Since the Nobel Prize winners Novoselov and Geim used mechanical exfoliation to separate single-layer graphene in 2004, a wave of research on the construction of new two-dimensional nanostructures has been set off. So far, the two-dimensional materials that have been constructed mainly include zero-bandgap graphene, wide-bandgap transition metal dichalcogenides (TMDCs), transition metal carbides (Mxenes), and transition metal oxides (such as MoO3, WO3, etc.), forming an emerging family of materials.

[0003] The interlayer coupling of two-dimensional layered materials is divided into weak interlayer coupling and strong interlayer coupling. Among them, the three-dimensional graphene material contains two kinds of carbon atoms with different properties in its primitive cell, which are sp 2 The hybridization method builds a strong σ interaction, and the interlayer p z The orbitals form weak van der Waals coupling through π-π stacking; there are only two unequal Dirac points in its band structure, so graphene is a zero-gap semiconductor material. It is precisely because of the unique band structure and electron type of graphene that it has excellent thermal and electrical properties. Studies have shown that its lattice thermal conductivity is as high as 5300W / (m·K), which can be used as an excellent heat sink; at the same time, it has a very high carrier mobility (up to 15000cm at room temperature). 2 / (V·s)), which is about 10 times higher than that of silicon-based materials; even up to 250,000 cm at low temperatures 2 / (V·s); and can induce magnetism through defect design or atomic adsorption.

[0004] Bi2O2X (X = S, Se, Te) is a representative of ternary layered bismuth oxygen chalcogenide compounds, a narrow-bandgap two-dimensional semiconductor material composed of positively charged [Bi2O2] 2+ With negative charge [X] 2- Compared with the highly symmetrical Bi2O2Se lattice, the lattices of Bi2O2S and Bi2O2Te are slightly distorted, which is manifested in the adjacent [Bi2O2] 2+The interlayer displacement and slight deformation of the Bi2O2Te lattice due to Te substitution, as well as the Rushba splitting in the Bi2O2Te energy bands, further indicate the violation of inversion symmetry.

[0005] As a thermoelectric material, the layered compound Bi2O2X has remarkable air stability, tunable band structure, high carrier mobility and responsiveness to various external signals. It has shown attractive application prospects in the fields of photocatalysis and high-performance optoelectronic devices, and is therefore considered a candidate material for a new generation of electronic devices. The layered material can achieve regulation of the material band structure and phonon dispersion length by adjusting the chemical composition, intrinsic nanostructure and defect structure; the material properties can be regulated by building a modular method to establish heterojunctions between adjacent layers; and the anisotropic chemical bonding state and local structural distortion in the layered crystal can also be studied through theoretical models.

[0006] Given the excellent properties of Bi2O2X two-dimensional materials, it is natural to expect that its corresponding one-dimensional materials should also have unique properties. Moreover, since one-dimensional nanowires have a larger surface-to-volume ratio, smaller size, one-dimensional carrier transport channels, and unique surface state properties, they will be more conducive to improving the performance of Bi2O2X one-dimensional materials. For example, a study successfully synthesized an oriented Bi2O2Se nanowire array using the CVD method, and found that the photodetector based on the Bi2O2Se nanowire array exhibited excellent performance in the ultraviolet to near-infrared spectrum, with a response rate, detection rate, external quantum efficiency, and response time of up to 722.2A / W, 5.64×10 11 Jones, 189000%, 0.267ms, these phenomena indicate that Bi2O2Se nanowire arrays have high crystallinity and surface trap states or defects, and have broad application prospects in the field of ultrafast and near-infrared photoelectric detection. Some studies have also successfully synthesized Bi2O2Se nanowires using the VLS method, and carried out low-temperature quantum transport research, observing gate-adjustable h / e periodic resistance oscillations, and attributed them to quasi-ballistic transport through the surface states of Bi2O2Se nanowires. The quasi-ballistic and phase-coherent surface states of Bi2O2Se nanowires confirmed by them provide an ideal platform for the design of future quantum electronics. Other studies have developed a catalyst-free CVD method to grow Bi2O2Se nanoribbons on mica substrates, and field-effect transistors made of Bi2O2Se nanoribbons exhibit n-type semiconductor characteristics with electron mobility as high as 262cm 2 / (V·s), switching ratio up to 10 7 In addition, the photoresponsivity of the Bi2O2Se nanoribbon photodetector is about 9.2×10 6 A / W, has a wide range of application potential.

[0007] One-dimensional materials refer to materials in which atoms grow in regular arrangement in one direction and only a few atoms are arranged in the other two directions, such as linear materials. Among them, Bi2O2Te crystals have a tetragonal structure and belong to the I4 / mmm space group. In the unit cell, each O atom covalently bonds with four Bi atoms to form a Bi4O tetrahedron. The tetrahedrons share edges and are arranged side by side to form a positively charged [Bi2O2] n 2n+ layer, and with the negatively charged [Te] n 2n- The layers are stacked alternately to form a layered structure. Bi2O2Te has ultra-high carrier mobility, a narrow band gap, good air stability, and sensitive responsiveness in ultraviolet, infrared and other bands. Based on the characteristics of one-dimensional materials, it can be inferred that Bi2O2Te one-dimensional materials have more unique properties, such as their larger surface-to-volume ratio, one-dimensional carrier transport channels and unique surface state properties, which will have strong competitiveness in the future field of micro-nanoelectronics. However, there are currently no reports on the synthesis and research of Bi2O2Te one-dimensional materials. In addition, the bismuth-based oxychalcogenide compounds of the same family as Bi2O2Te include Bi2TeO5, whose crystals have a non-centrosymmetric structure and contain Bi 3+ and Te 4+ , and contains lone pairs of electrons in strongly twisted oxygen coordination polyhedra. Studies have reported that Bi2O2Te is a dielectric and piezoelectric material with a high dielectric constant. At the same time, Bi2TeO5 is also a nonlinear optical material with interesting properties. Its crystals show long-lived photorefractive signals and obvious nonlinear light absorption effects. There are also no reports on the synthesis and research of Bi2TeO5 one-dimensional materials.

[0008] The VLS method is a combined material preparation method. In the growth system, there are three states of matter: gas, liquid, and solid. The material to be grown first changes from solid to gas, then gathers in the catalyst droplets together with the gas, and then grows crystals by solid deposition on the crystal substrate. Therefore, if Bi2O2Te / Bi2TeO5 one-dimensional materials can be prepared by the VLS method, it will have broad application prospects. Summary of the invention

[0009] In order to overcome the above-mentioned deficiencies of the prior art, the present invention proposes a method for growing Bi2O2Te / Bi2TeO5 one-dimensional materials on thermally evaporated gold silicon wafers or drop-coated gold silicon wafers using the VLS method, which fills the gap in zero synthesis of Bi2O2Te / Bi2TeO5 one-dimensional materials.

[0010] In order to achieve the above object, the technical solution adopted by the present invention is:

[0011] The present invention provides a controllable synthesis and preparation method of a bismuth-based oxychalcogenide (Bi2O2Te / Bi2TeO5) one-dimensional material, which specifically comprises the following steps: using a heat-evaporated gold silicon wafer or a drop-coated gold silicon wafer as a substrate and Bi2Te3 powder as a precursor, placing the heat-evaporated gold silicon wafer or the drop-coated gold silicon wafer at a heating center of a growth zone located downstream of a double-temperature zone tubular furnace, and placing the Bi2Te3 powder at a heating center of a raw material zone located upstream of the double-temperature zone tubular furnace, first reducing the pressure in the tubular furnace to 0Pa, then heating the heating center of the raw material zone and the heating center of the growth zone to target temperatures respectively and simultaneously, then introducing high-purity argon or a mixed gas of high-purity argon and high-purity oxygen, and continuing to maintain the pressure in the tube at 0Pa all the time, and then naturally cooling to room temperature after maintaining for 4-6 hours.

[0012] Preferably, the thickness of the gold nanoparticle layer plated on the thermally evaporated gold silicon wafer is 8 nm, the particle size of the gold particles on the drop-coated gold silicon wafer is 50 nm, the distance between the thermally evaporated gold silicon wafer or the drop-coated gold silicon wafer and the Bi2Te3 powder is 10 cm, and when high-purity argon gas is introduced, a Bi2O2Te one-dimensional material is prepared.

[0013] Preferably, when the gold particle size on the gold-coated silicon wafer is 5 nm or 50 nm, the distance between the gold-coated silicon wafer and the Bi2Te3 powder is 10 cm, and a mixed gas of high-purity argon and high-purity oxygen is introduced at the same time, a Bi2TeO5 one-dimensional material is prepared.

[0014] The entire reaction process of the present invention is roughly divided into two steps: (1) gaseous reactants and carrier gas gather in catalyst gold particle droplets; (2) product precursors reach supersaturation in the catalyst and precipitate along the direction of the lowest solid-liquid interface energy (perpendicular to the interface) at the solid-liquid interface, thereby growing a one-dimensional material. The method of the present invention has a simple preparation process, simple preparation materials, low preparation temperature, good controllability, and can control the density of Bi2O2Te / Bi2TeO5 one-dimensional materials by controlling conditions such as the substrate, and successfully synthesizes Bi2O2Te / Bi2TeO5 one-dimensional materials.

[0015] Preferably, the target temperatures of the heating center of the feed zone and the heating center of the growth zone are 570-590°C and 520-540°C, respectively.

[0016] More preferably, the target temperatures of the heating center of the feed zone and the heating center of the growth zone are 580°C and 530°C, respectively.

[0017] Preferably, the time required to heat the heating center of the raw material zone and the heating center of the growth zone to the target temperature is no more than 37 minutes.

[0018] Preferably, the amount of high-purity argon gas introduced is 380-420 sccm, and the amount of high-purity oxygen gas introduced is 4-6 sccm.

[0019] More preferably, the amount of high-purity argon gas introduced is 400 sccm, and the amount of high-purity oxygen gas introduced is 5 sccm.

[0020] Preferably, the method for preparing the thermally evaporated gold silicon wafer is: using a thermal evaporation method to plate a layer of gold nanoparticles on the surface of the silicon wafer.

[0021] Preferably, the preparation method of the drop-coated gold silicon wafer is: drop-coating the gold particle dispersion on the surface of the silicon wafer and drying it naturally.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention discloses a method for controllably synthesizing Bi2O2Te / Bi2TeO5 one-dimensional materials based on a VLS method. First, a certain mass of Bi2Te3 powder is weighed as a precursor and placed in a high temperature zone, and a thermally evaporated gold silicon wafer or a drop-coated gold silicon wafer is used as a substrate and placed in a low temperature zone. After vacuuming, the temperatures of the two temperature zones are raised to a target temperature at a certain rate, and then a carrier gas is introduced to grow the one-dimensional material. After the growth is completed, the carrier gas is stopped, and the material is naturally cooled to room temperature, so that the Bi2O2Te / Bi2TeO5 one-dimensional material is prepared. The method of the invention has a simple preparation process, simple preparation materials, low temperature during preparation, good controllability, and the density of the Bi2O2Te / Bi2TeO5 one-dimensional material can be controlled by controlling conditions such as the substrate. It can be seen that the invention has the advantages of simple operation, high safety, strong controllability, etc., and fills the blank of zero synthesis of Bi2O2Te / Bi2TeO5 one-dimensional materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of growing Bi2O2Te / Bi2TeO5 one-dimensional materials on thermally evaporated gold silicon wafer or drop-coated gold silicon wafer using VLS method, wherein: 1-tube furnace, 2-Bi2Te3 powder, 3-quartz boat, 4-thermally evaporated gold silicon wafer or drop-coated gold silicon wafer, 5-quartz wafer;

[0025] Figure 2 , 5 XRD spectrum of the prepared Bi2O2Te one-dimensional material;

[0026] Figure 3 , 6 This is the SEM image of the prepared Bi2O2Te one-dimensional material;

[0027] Figure 4 , 7 This is the EDS image of the prepared Bi2O2Te one-dimensional material;

[0028] Figure 8 , 11 This is the XRD spectrum of the prepared Bi2TeO5 one-dimensional material;

[0029] Fig. 9 , 12 This is the SEM image of the prepared Bi2TeO5 one-dimensional material;

[0030] Fig.10 , 13 This is the EDS image of the prepared Bi2TeO5 one-dimensional material. DETAILED DESCRIPTION

[0031] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0032] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0033] Example 1 Preparation of Bi2O2Te one-dimensional material

[0034] like Figure 1 As shown, the preparation of Bi2O2Te one-dimensional material includes the following steps:

[0035] (1) Base

[0036] A thermally evaporated gold-deposited silicon wafer with a size of about 1cm×1cm was selected as the substrate: the silicon wafer was first repeatedly cleaned with anhydrous ethanol and deionized water, and blown dry with a hair dryer, and then a layer of gold nanoparticles with a thickness of about 8nm was vacuum evaporated on the surface of the clean silicon wafer to obtain the substrate required for growth, and finally the substrate was placed on a quartz wafer.

[0037] (2) Precursor

[0038] Place the weighing paper on the electronic balance and perform the tare operation; use a medicine spoon to place the Bi2Te3 powder on the weighing paper and weigh 2g; pour the weighed Bi2Te3 powder into a clean quartz boat.

[0039] (3) Preparation

[0040] A dual-temperature zone tubular furnace (NBD-01200) was selected to grow bismuth-based oxysulfide one-dimensional materials using the VLS method. The quartz boat of step (2) was placed at the heating center of the raw material zone upstream of the tubular furnace, and the quartz sheet of step (1) was placed at the heating center of the growth zone downstream of the tubular furnace, and the substrate of step (1) was about 10 cm away from the precursor of step (2) (i.e., Bi2Te3 powder); then, the inlet and outlet valves and the vacuum pump were opened to reduce the pressure in the tubular furnace to 0 Pa, and then the inlet and outlet valves were closed, and the heating switch was turned on, so that the heating centers of the raw material zone and the growth zone were simultaneously heated to 580°C and 530°C, respectively, within 37 minutes.

[0041] (4) Growth of Bi2O2Te one-dimensional materials

[0042] 400 sccm of high-purity argon gas was introduced, and the inlet and outlet valves and the vacuum pump were opened at the same time to maintain the pressure in the tube at 0 Pa, and maintained for 5 hours; finally, the gas and the inlet valve were closed to maintain the pressure in the tube at 0 Pa, and the outlet valve and the vacuum pump were closed, and the substrate was taken out after naturally cooling to room temperature.

[0043] (5) Results characterization

[0044] The grown sample was characterized by XRD, and the spectrum obtained was Figure 2 ,Depend on Figure 2 It can be seen that the peak of the sample corresponds well to the standard spectrum peak of Bi2O2Te. At the same time, the grown substrate is placed under SEM for observation, and the results are as follows Figure 3 As shown in the figure, it can be seen that some linear materials have grown, with a size of about 30μm×0.3μm. In addition, the element ratio of the grown sample was tested by EDS. Figure 4 The EDS graph shows that Bi:O:Te=1.92:2.33:1, which is roughly consistent with the element ratio of Bi2O2Te. The above results show that the Bi2O2Te one-dimensional material was successfully prepared in this embodiment.

[0045] Example 2 Preparation of Bi2O2Te one-dimensional material

[0046] The preparation method is the same as that in Example 1, except that the substrate in step (1) is a gold-coated silicon wafer on which gold particles with a particle size of about 50 nm are drop-coated: the silicon wafer is repeatedly cleaned with anhydrous ethanol and deionized water and dried with a hair dryer, and a 50 nm gold particle dispersion is drop-coated on the clean silicon wafer surface and naturally dried to obtain the substrate required for growth.

[0047] The grown sample was characterized by XRD, and the spectrum obtained was Figure 5 ,Depend on Figure 5It can be seen that the peak of the sample corresponds well to the standard spectrum peak of Bi2O2Te. At the same time, the grown substrate is placed under SEM for observation, and the results are as follows Figure 6 As shown in the figure, it can be seen that some linear materials have grown, with a size of about 30μm×0.3μm. In addition, the element ratio of the grown sample was tested by EDS. Figure 7 The EDS graph shows that Bi:O:Te=2.01:2.02:1, which is roughly consistent with the element ratio of Bi2O2Te. The above results show that the one-dimensional Bi2O2Te material is successfully prepared in this embodiment.

[0048] Example 3 Preparation of Bi2TeO5 one-dimensional material

[0049] The preparation method is the same as that of Example 1, except that, when growing the one-dimensional material in step (4), not only 400 sccm of high-purity argon but also 5 sccm of high-purity oxygen is introduced, and the substrate of step (1) is a gold-coated silicon wafer on which gold particles with a particle size of about 5 nm are deposited.

[0050] The grown sample was characterized by XRD, and the spectrum obtained was Figure 8 ,Depend on Figure 8 It can be seen that the peak of the sample corresponds well to the standard spectrum peak of Bi2TeO5. At the same time, the grown substrate is placed under SEM for observation, and the results are as follows Fig. 9 As shown in the figure, it can be seen that some linear materials have grown, with a size of about 10μm×0.5μm. In addition, the element ratio of the grown sample was tested by EDS. Fig.10 The EDS graph shows that Bi:Te=2.18:1, which is roughly consistent with the element ratio of Bi2TeO5. The above results show that the one-dimensional Bi2TeO5 material was successfully prepared in this embodiment.

[0051] Example 4 Preparation of Bi2TeO5 one-dimensional material

[0052] The preparation method is the same as that of Example 1, except that, when growing the one-dimensional material in step (4), not only 400 sccm of high-purity argon but also 5 sccm of high-purity oxygen is introduced, and the substrate of step (1) is a gold-coated silicon wafer on which gold particles with a particle size of about 50 nm are deposited.

[0053] The grown sample was characterized by XRD, and the spectrum obtained was Fig.11 ,Depend on Fig.11 It can be seen that the peak of the sample corresponds well to the standard spectrum peak of Bi2TeO5. At the same time, the grown substrate is placed under SEM for observation, and the results are as follows Fig.12As shown in the figure, it can be seen that some linear materials have grown, with a size of about 10μm×0.5μm. In addition, the element ratio of the grown sample was tested by EDS. Fig.13 The EDS graph shows that Bi:Te=1.78:1, which is roughly consistent with the element ratio of Bi2TeO5. The above results show that the one-dimensional Bi2TeO5 material is successfully prepared in this embodiment.

[0054] Comparative Example 1

[0055] The preparation method is the same as that of Example 1, except that the substrate in step (1) is a silicon wafer with a size of about 1 cm×1 cm.

[0056] The grown substrate was placed under SEM for observation and no product was found.

[0057] Comparative Example 2

[0058] The preparation method is the same as that of Example 1, except that the substrate in step (1) is fluorophlogopite with a size of about 1 cm×1 cm.

[0059] The grown substrate was placed under SEM for observation and no product was found.

[0060] In summary, the present invention successfully grows Bi2O2Te / Bi2TeO5 one-dimensional materials on thermally evaporated gold silicon wafers or drop-coated gold silicon wafers using the VLS method. Moreover, the growth and density of the Bi2O2Te / Bi2TeO5 one-dimensional materials obtained by the present invention are closely related to the substrate. In the synthesis of Bi2O2Te one-dimensional materials, the density of the one-dimensional material grown using a thermally evaporated gold substrate is larger than that of the drop-coated substrate, and the size is about 30μm×0.3μm, while there is no product from silicon wafers and fluorphlogopite without thermally evaporated gold or drop-coated gold; in the synthesis of Bi2TeO5 one-dimensional materials, the density of the one-dimensional material grown using a drop-coated 50nm gold particle substrate is larger than that of a drop-coated 5nm gold particle substrate, and the size is about 10μm×0.5μm. At the same time, the prepared Bi2O2Te / Bi2TeO5 one-dimensional material was tested for its element ratio using EDS, and the results showed that it was roughly consistent with the element ratio of Bi2O2Te / Bi2TeO5. In addition, XRD was used to characterize the phase transition of the grown material. Bi2Te3 had multiple strong peaks at 2θ=17.32, 27.54, 37.68, 44.42, etc., corresponding to (00-6), (015), (-1110), (00-15), etc. After growth, multi-peak Bi2O2Te phase transition occurred at 2θ=14.02, 23.44, 28.18, 30.86, 31.80, 42.78, 45.54, 54.24, 54.40, 55.7, 56.02, 58.18, 64.24, corresponding to (002), (011), (004), (013), (110), (006), (020), (116), (024), (017 ), (123), (008), (026); multi-peak Bi2TeO5 phase transition occurred at 2θ=7.68, 10.78, 15.34, 23.07, 27.64, 30.90, 32.70, 38.90, 45.52, 64.39, corresponding to (100), (020), (200), (211), (231), (400), (151), (500), (460), (800), respectively. The above results show that the Bi2O2Te / Bi2TeO5 one-dimensional material was successfully synthesized.

[0061] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. Bi 2 TeO 5 Controllable synthesis and preparation method of one-dimensional materials, It is characterized in that Using thermally evaporated gold silicon wafer or drop-coated gold silicon wafer as the substrate, Bi 2 Te 3 Powder is used as a precursor, and a hot evaporated gold-deposited silicon wafer or a drop-coated gold-deposited silicon wafer is placed in the heating center of the growth zone downstream of the dual-temperature zone tube furnace, and Bi 2 Te 3 The powder is placed in the heating center of the raw material zone located upstream of the dual-temperature zone tubular furnace. The pressure in the tubular furnace is first reduced to 0 Pa, and then the heating center of the raw material zone and the heating center of the growth zone are heated to the target temperature at the same time. The target temperatures of the heating center of the raw material zone and the heating center of the growth zone are 570-590 °C and 520-540 °C, respectively. Then, a mixed gas of high-purity argon and high-purity oxygen is introduced, and the pressure in the tube is maintained at 0 Pa. After maintaining for 4-6 hours, it is naturally cooled to room temperature. When the gold particle size on the drop-coated gold silicon wafer is 5 nm or 50 nm, the distance between the drop-coated gold silicon wafer and Bi 2 Te 3 When the distance between the powder and the sample was 10 cm and a mixture of high-purity argon and high-purity oxygen was introduced at the same time, Bi 2 TeO 5 One-dimensional material.

2. Bi according to claim 1 2 TeO 5 Controllable synthesis and preparation method of one-dimensional materials, It is characterized in that The target temperatures of the heating center of the feed zone and the heating center of the growth zone are 580 °C and 530 °C, respectively.

3. Bi according to claim 1 2 TeO 5 Controllable synthesis and preparation method of one-dimensional materials, It is characterized in that The time for heating the heating center of the raw material zone and the heating center of the growth zone to reach the target temperature is no more than 37 minutes.

4. Bi according to claim 1 2 TeO 5 Controllable synthesis and preparation method of one-dimensional materials, It is characterized in that The amount of high-purity argon gas introduced is 380-420 sccm, and the amount of high-purity oxygen gas introduced is 4-6 sccm.