A method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid

Through chemical precipitation method and acid treatment technology, combined with iron salt and ammonium source reaction, the vanadium and arsenic were successfully separated in high-concentration alkali liquid, solving the complex separation problem of vanadium and arsenic, achieving efficient recycling of vanadium and deep removal of arsenic , reducing treatment costs and reagent consumption.

CN116443926BActive Publication Date: 2024-11-29INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202310569047.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

The prior art is difficult to effectively separate vanadium and arsenic in high concentration alkaline liquids, and the traditional wet alkali leach recovery method has complex components and high cost problems of vanadium and arsenic.

Method used

The vanadium and arsenic waste liquid is mixed with calcium salt by chemical precipitation. After precipitation, the acid treatment and iron salt are separated. Finally, the ammonium polyvanadate is reacted with the ammonium source to prepare ammonium polyvanadate to achieve selective separation and recovery of vanadium and arsenic.

Benefits of technology

The selective separation of vanadium and arsenic in high concentration alkali liquid is achieved, the treatment cost is reduced, the recovery rate of vanadium and arsenic removal rate is improved, and the process is simple, the reagent consumption is low, and there is no waste gas generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116443926B_ABST
    Figure CN116443926B_ABST
Patent Text Reader

Abstract

The present invention provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, the method comprising: (1) mixing the vanadium-arsenic waste liquid with a precipitant, and obtaining a precipitate containing vanadium and arsenic after reaction; (2) subjecting the precipitate containing vanadium and arsenic to acid treatment to obtain an acidic solution containing vanadium and arsenic; (3) mixing the acidic solution containing vanadium and arsenic with an arsenic separation agent, and separating arsenic after reaction to obtain a vanadium-containing solution; (4) mixing the vanadium-containing solution with an ammonium source, and reacting to obtain the ammonium polyvanadate. The present invention adopts a short-process, high-efficiency chemical precipitation method under mild conditions, which can not only realize the selective recovery of strategic metal vanadium resources, but also realize the reuse of high-concentration alkaline solutions and acid leaching solutions, thereby avoiding the waste of valuable metal resources, reducing the wastewater discharge of the entire process, and alleviating the environmental pollution problem caused by the discharge of toxic heavy metal wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary resource utilization, and relates to a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, and in particular to a method for selectively preparing ammonium polyvanadate from high-concentration vanadium-arsenic waste liquid. Background Art

[0002] As an important strategic resource, vanadium is widely used in the fields of steel, chemical industry, aerospace, military industry and new energy. The output of vanadium mainly comes from three sources: direct vanadium extraction from minerals such as vanadium-titanium magnetite, vanadium extraction from vanadium slag obtained by steel metallurgical processing of vanadium-titanium magnetite, and vanadium extraction from secondary recycled vanadium-containing waste. Among them, there are many types of vanadium-containing waste, including vanadium-containing steel slag, vanadium extraction tailings, deactivated catalysts, and vanadium battery failed electrolytes. Recycling vanadium-containing waste as a secondary resource can not only bring higher economic and environmental benefits, but also has important significance for the recycling of resources. For example, the production of vanadium-based catalysts represented by waste denitrification (SCR) catalysts is increasing year by year. The vanadium content in waste SCR catalysts is above 0.5%, and the annual recovery volume is expected to reach 3,000 tons (in terms of V2O5), which has a very high recovery value. Therefore, from the perspective of environmental safety and comprehensive resource utilization, it is of great significance and high economic value to study the selective recovery of metallic vanadium from vanadium-containing waste.

[0003] Compared with the traditional high-temperature roasting recovery, the wet alkaline leaching recovery method has the advantages of high vanadium leaching rate, mild leaching conditions, and fewer types of impurity ions in the leachate, and has attracted widespread attention. However, since vanadium and arsenic elements are both transition metals and have similar electronic layer structures, they also show similar leaching behaviors in high-concentration alkaline solutions. Therefore, in the wet alkaline leaching recovery of vanadium, a high-concentration vanadium-arsenic mixed alkaline solution is usually produced (the concentration of vanadium or arsenic can reach 6-10g / L, and the pH is about 13). At present, the selective separation of valuable metal elements such as vanadium, tungsten, and arsenic in the solution is mostly achieved by adsorption, extraction, and membrane separation, but it is not suitable for concentrated alkaline systems with excessively high metal ion concentrations and complex components. Therefore, it is urgent to develop a new treatment process with short process, high efficiency, and low cost.

[0004] CN112553469B discloses a method for separating vanadium, tungsten and arsenic from sodium hydroxide waste liquid. The method utilizes the difference in solubility of metal sodium salts corresponding to elements such as tungsten, vanadium and arsenic under different alkali concentrations, and can separate tungsten from the solution by adjusting the NaOH concentration and performing two causticizing reactions. The separation efficiency of tungsten is more than 90%. However, the method is difficult to effectively separate vanadium and arsenic in the alkali solution.

[0005] CN104492421B discloses a method for removing arsenic from a catalyst containing tungsten, vanadium and arsenic. The method can increase the arsenic removal rate to 95% by adding Ca(OH)2 to the alkaline leaching solution, but a large amount of vanadium precipitation will also be produced. In order to further reduce the loss of vanadium and tungsten in the solution, it is necessary to add inhibitors EDTA and ammonium bicarbonate to the solution while removing arsenic, which not only introduces new impurity ions, but also the vanadium loss rate can reach 30%.

[0006] CN113430381A discloses a method for harmless treatment of arsenic-containing waste SCR denitration catalyst. The method uses a composite extractant to selectively recover a mixed solution of vanadium and arsenic. Although the method can achieve effective separation and recovery of arsenic and vanadium, it also has the disadvantages of long pretreatment steps, large reagent consumption, and the need for an additional stripping step.

[0007] Therefore, it is urgent to develop a simple and efficient treatment process that can achieve efficient extraction of vanadium and deep removal of arsenic in high-concentration alkali solution, as well as recycling and reuse of alkali solution. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid. The method of the present invention can simultaneously achieve the selective separation of vanadium-arsenic elements in high-concentration alkaline solution, the recovery of high-value products of valuable vanadium elements and the harmless treatment of toxic arsenic elements, thereby achieving the purpose of clean production. In addition, the present invention first uses a precipitant to treat the vanadium-arsenic waste liquid, and can achieve the recovery of the vanadium-arsenic alkaline separation liquid through simple evaporation and crystallization, which can effectively reduce the cost of recovering vanadium-containing waste by wet alkaline leaching.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] The present invention provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, the method comprising:

[0011] (1) mixing vanadium-arsenic waste liquid and a precipitant to obtain a precipitate containing vanadium and arsenic after reaction;

[0012] (2) treating the precipitate containing vanadium and arsenic with acid to obtain an acidic solution containing vanadium and arsenic;

[0013] (3) mixing the acidic solution containing vanadium and arsenic with an arsenic separation agent, separating arsenic after reaction, and obtaining a vanadium-containing solution;

[0014] (4) mixing the vanadium-containing solution and an ammonium source to react and obtain the ammonium polyvanadate.

[0015] The invention provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, which separates vanadium and arsenic by chemical precipitation treatment, and can realize the selective separation of vanadium and arsenic in high-concentration alkali liquid and the product recovery of vanadium element. The method of the invention is simple and direct, and the conditions are mild; the whole process has a short reaction time, a small overall consumption of reagents, and no waste gas is generated; the amount of waste water generated is small, and the types of anions and cations introduced in the whole process route are small, so that the impurity ions in the circulating alkali liquid are small.

[0016] In the present invention, vanadium-arsenic waste liquid and a precipitant are mixed, and after the reaction, not only a precipitate containing vanadium and arsenic is obtained, but also an alkaline separation liquid after separation of the precipitate can be obtained. The separation liquid can be reused in the process of wet alkaline treatment of vanadium-containing catalysts after evaporation and concentration, thereby reducing the overall treatment cost.

[0017] Preferably, the precipitant in step (1) comprises a calcium salt.

[0018] In the present invention, after the calcium salt is mixed with the vanadium-arsenic waste liquid for reaction, the obtained vanadium-and-arsenic-containing precipitate is a co-precipitate of calcium vanadate and calcium arsenate. The vanadium and arsenic in the vanadium-arsenic waste liquid are removed from the high-alkali solution in the form of insoluble calcium vanadate and calcium arsenate, and the precipitation rate can reach more than 99%, which is conducive to the recovery of the alkali solution.

[0019] Preferably, the calcium salt includes at least one of calcium oxide, calcium hydroxide, calcium chloride and calcium sulfate.

[0020] Preferably, the ratio of the molar amount of calcium in the calcium salt to the total molar amount of vanadium and arsenic in the vanadium-arsenic waste liquid is (1-6):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1 or 6:1.

[0021] In the present invention, when the molar amount of calcium in the calcium salt is too small to the total molar amount of vanadium and arsenic in the vanadium-arsenic waste liquid, it will lead to incomplete precipitation of vanadium, arsenic and other elements in the waste liquid; when the molar amount of calcium in the calcium salt is too large to the total molar amount of vanadium and arsenic in the vanadium-arsenic waste liquid, it will lead to the formation of Ca3(VO4)2, introduce too many calcium ions, and cause a large amount of calcium sulfate solid waste to be generated in the subsequent acid treatment stage.

[0022] Preferably, the reaction temperature in step (1) is 25-90°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, etc.

[0023] Preferably, the reaction time of step (1) is 2-3 h, for example, it can be 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h, 2.9 h or 3 h.

[0024] Preferably, the reaction process in step (1) is accompanied by stirring.

[0025] Preferably, in step (1), filtration is performed after the reaction to obtain the precipitate and filtrate containing vanadium and arsenic.

[0026] Preferably, the total mass concentration of vanadium and arsenic in the filtrate is 0.5-60 mg / L, for example, it can be 0.5 mg / L, 0.7 mg / L, 1 mg / L, 2 mg / L, 5 mg / L, 10 mg / L, 20 mg / L, 30 mg / L, 40 mg / L, 50 mg / L or 60 mg / L, etc.

[0027] Preferably, the pH value of the filtrate is 13-14, for example, it can be 13.1, 13.2, 13.3, 13.4, 13.5, 13.6, 13.7, 13.8, 13.9 or 14, etc.

[0028] In the present invention, the filtrate obtained in step (1) has low vanadium and arsenic contents and high basicity, and can be reused as crude floating alkali through evaporation and crystallization, and can also be used as an alkali leaching agent.

[0029] Preferably, the acid used in the acid treatment in step (2) comprises a sulfuric acid solution.

[0030] In the present invention, the precipitate containing vanadium and arsenic is treated with sulfuric acid solution to obtain calcium sulfate filter residue and an acidic mixed solution containing vanadium and arsenic.

[0031] Preferably, the mass fraction of the sulfuric acid solution is 8-13%, for example, 8%, 9%, 10%, 11%, 12% or 13%.

[0032] Preferably, the ratio of the mass of the vanadium- and arsenic-containing precipitate to the volume of the sulfuric acid solution is 1g:(5-20)mL, for example, it can be 1g:5mL, 1g:6mL, 1g:7mL, 1g:8mL, 1g:9mL, 1g:10mL, 1g:12mL, 1g:14mL, 1g:16mL, 1g:18mL or 1g:20mL, etc.

[0033] Preferably, the acid treatment method in step (2) specifically comprises: mixing the precipitate containing vanadium and arsenic with an acid to react.

[0034] Preferably, in the acid treatment method, the reaction temperature is 25-80°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.

[0035] Preferably, in the acid treatment method, the reaction time is 2-3 h, for example, it can be 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h, 2.9 h or 3 h.

[0036] Preferably, in the acid treatment method, the reaction process is accompanied by stirring.

[0037] Preferably, the pH value of the acidic solution containing vanadium and arsenic in step (2) is 1-3, for example, it can be 1, 1.2, 1.5, 1.7, 2, 2.2, 2.5, 2.7 or 3.

[0038] Preferably, the arsenic separation agent in step (3) comprises an iron salt.

[0039] In the present invention, in order to further separate arsenic in the precipitate and recover vanadium, arsenic is converted into harmless ferric arsenate precipitate by adding iron salt after dissolving it in sulfuric acid. Arsenic is separated in the form of ferric arsenate precipitate, and the comprehensive removal rate of arsenic can reach 93.74%.

[0040] Preferably, the iron salt includes at least one of ferric chloride, ferrous chloride, ferric sulfate and ferrous sulfate.

[0041] Preferably, the ratio of the molar amount of iron in the iron salt to the molar amount of arsenic in the acidic solution containing vanadium and arsenic is (1-3):1, for example, it can be 1:1, 1.2:1, 1.5:1, 1.7:1, 2:1, 2.2:1, 2.5:1, 2.7:1 or 3:1, etc.

[0042] In the present invention, when the ratio of the molar amount of the iron element in the iron salt to the molar amount of the arsenic element in the acidic solution containing vanadium and arsenic is too small, it will lead to incomplete arsenic precipitation and incomplete vanadium-arsenic separation; when the ratio of the molar amount of the iron element in the iron salt to the molar amount of the arsenic element in the acidic solution containing vanadium and arsenic is too large, it will lead to the generation of insoluble iron vanadate, resulting in a waste of vanadium resources.

[0043] Preferably, in step (3), before the mixing, the pH value of the acidic solution containing vanadium and arsenic is adjusted to 2-3.5, for example, 2, 2.1, 2.4, 2.5, 2.6, 2.7, 2.9, 3, 3.2 or 3.5, and an oxidation step is performed.

[0044] Preferably, an alkali solution is used to adjust the pH value of the acidic solution containing vanadium and arsenic.

[0045] Preferably, the alkali solution comprises a NaOH solution, and the concentration of the NaOH solution is 0.1-1M, for example, it can be 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, 0.6M, 0.7M, 0.8M, 0.9M or 1M, etc.

[0046] Preferably, the oxidation step specifically comprises: mixing an acidic solution containing vanadium and arsenic with an adjusted pH value with an oxidant to carry out an oxidation reaction.

[0047] In the present invention, the oxidation reaction is carried out to oxidize the arsenic element in the acidic solution containing vanadium and arsenic to the highest valence state, which is helpful for the subsequent precipitation reaction and is conducive to separating the arsenic element.

[0048] Preferably, the oxidant comprises H2O2.

[0049] Preferably, the ratio of the molar amount of the H2O2 to the total molar amount of the vanadium element and the arsenic element in the acidic solution containing vanadium and arsenic is (1-4):1, for example, it can be 1:1, 1.2:1, 1.5:1, 1.7:1, 2:1, 2.2:1, 2.5:1, 2.7:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1 or 4:1, etc.

[0050] Preferably, the oxidation reaction time is 30-60 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0051] Preferably, the reaction temperature in step (3) is 25-40°C, for example, it can be 25°C, 27°C, 29°C, 30°C, 32°C, 34°C, 35°C, 37°C, 39°C or 40°C.

[0052] Preferably, the reaction time of step (3) is 2-3 h, for example, it can be 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h, 2.9 h or 3 h.

[0053] Preferably, the reaction process in step (3) is accompanied by stirring.

[0054] Preferably, the ammonium source in step (4) comprises an ammonium salt.

[0055] In the present invention, the introduction of ammonium salt enables vanadium to be recovered in the form of ammonium vanadate product, and the comprehensive recovery rate of vanadium can reach more than 90%.

[0056] Preferably, the ammonium salt comprises ammonium chloride and / or ammonium sulfate.

[0057] Preferably, the ammonium ion (NH4 +) to the molar amount of vanadium element in the vanadium-containing solution is (0.33-0.4):1, for example, it can be 0.33:1, 0.34:1, 0.35:1, 0.36:1, 0.37:1, 0.38:1, 0.39:1 or 0.4:1, etc.

[0058] Preferably, in step (4), after the vanadium-containing solution and the ammonium source are mixed, the pH value of the obtained mixed solution is adjusted to 1.9-2.3, for example, 1.9, 2, 2.1, 2.2 or 2.3.

[0059] Optionally, an acid or a base is used to adjust the pH value of the mixed solution.

[0060] Preferably, the reaction temperature in step (4) is 80-100°C, for example, it can be 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C or 100°C, etc.

[0061] Preferably, the reaction time of step (4) is 0.5-3 h, for example, it can be 0.5 h, 0.7 h, 0.9 h, 1 h, 1.2 h, 1.5 h, 1.7 h, 2 h, 2.2 h, 2.5 h, 2.7 h or 3 h.

[0062] Preferably, the reaction process in step (4) is accompanied by stirring.

[0063] Preferably, in step (4), filtration is performed after the reaction to obtain the ammonium polyvanadate precipitate product and a clear liquid.

[0064] Preferably, the concentration of vanadium in the clear solution is less than 0.2 g / L, for example, it can be 0.19 g / L, 0.18 g / L, 0.17 g / L, 0.16 g / L, 0.15 g / L, 0.13 g / L, 0.12 g / L, 0.1 g / L, 0.07 g / L or 0.05 g / L, etc.

[0065] As a preferred technical solution of the present invention, the method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid specifically comprises:

[0066] (I) adding calcium salt to vanadium-arsenic waste liquid, reacting at 25-90° C. for 2-3 hours, and filtering to obtain a co-precipitate of calcium vanadate and calcium arsenate and a filtrate, wherein the total mass concentration of vanadium and arsenic in the filtrate is 0.5-60 mg / L;

[0067] (II) adding a sulfuric acid solution to the calcium vanadate and calcium arsenate coprecipitate, reacting at 25-80° C. for 2-3 hours, and filtering to obtain an acidic solution containing vanadium and arsenic and a calcium sulfate filter residue, wherein the pH value of the acidic solution containing vanadium and arsenic is 1-3;

[0068] (III) using alkaline solution to adjust the pH value of the acidic solution containing vanadium and arsenic to 2-3.5, then adding H2O2 to the acidic solution containing vanadium and arsenic with adjusted pH value, and performing oxidation reaction for 30-60 minutes, then adding iron salt to the oxidized acidic solution containing vanadium and arsenic, reacting at 25-40°C for 2-3 hours, and then filtering to obtain iron arsenate residue and vanadium-containing solution, wherein the pH value of the vanadium-containing solution is 2-4;

[0069] (IV) adding an ammonium source to the vanadium-containing solution, adjusting the pH value of the obtained mixed solution to 1.9-2.3, reacting at 80-100° C. for 0.5-3 h, and filtering to obtain the ammonium polyvanadate and a clear solution, wherein the concentration of vanadium in the clear solution is less than 0.2 g / L.

[0070] In the present invention, first, after adding calcium salt, vanadium and arsenic in the solution are removed from the high alkali solution in the form of insoluble calcium vanadate and calcium arsenate, and the precipitation rate can reach more than 99%, so that the alkali solution can be recovered. In order to further separate the arsenic in the coprecipitate and recover the vanadium element, the arsenic is converted into iron arsenate precipitation by adding iron salt after dissolving it in sulfuric acid, and the comprehensive removal rate of arsenic can reach 93.74%; finally, the introduction of ammonium salt allows the vanadium to be recovered in the form of ammonium vanadate product, and the comprehensive recovery rate of vanadium can reach more than 90%. The whole process has a short reaction time, a small overall consumption of reagents, and no waste gas is generated; the amount of wastewater generated is small, and the waste residue is harmless calcium sulfate and iron arsenate (scoralite).

[0071] The method of the present invention has obvious advantages. First, the types of anions and cations introduced in the whole process route are small, mainly Na + , Ca 2+ , Fe 2+ / Fe 3+ and SO4 2- ; Secondly, the main waste residue produced by this process is calcium sulfate, which has low vanadium and arsenic content and can be further processed as gypsum raw material; finally, this process produces a small amount of wastewater, most of the filtrate is the raw material for the next stage or can be reused, and no waste gas is generated.

[0072] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0073] Compared with the prior art, the present invention has the following beneficial effects:

[0074] The present invention provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, which uses a chemical precipitation treatment method to separate vanadium and arsenic, and can achieve the selective separation of vanadium and arsenic in high-concentration alkali liquid and the product recovery of vanadium element, and has the advantages of being simple, direct, and mild. The whole process has a short reaction time, a small amount of reagent consumption, and no waste gas is generated; the amount of waste water generated is small, and the types of anions and cations introduced in the whole process route are small, so that the impurity ions are small;

[0075] In the present invention, the vanadium-arsenic waste liquid and the precipitant are mixed, and after the reaction, not only a precipitate containing vanadium and arsenic is obtained, but also an alkaline separation liquid after the precipitate is separated can be obtained. The separation liquid can be recycled to reduce the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 A schematic diagram of a process for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0077] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0078] In one embodiment, the present invention provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, such as Figure 1 As shown, the method comprises the following steps:

[0079] (1) adding calcium salt to vanadium-arsenic waste liquid for precipitation reaction, and obtaining a precipitate containing vanadium and arsenic and an alkaline solution through filtration, wherein the precipitate containing vanadium and arsenic is a co-precipitate of calcium vanadate and calcium arsenate, and the alkaline solution can be reused in the process of wet leaching of vanadium-containing waste;

[0080] (2) adding an acid-soluble reagent to the precipitate containing vanadium and arsenic, and filtering to obtain calcium sulfate and an acidic solution containing vanadium and arsenic after the reaction;

[0081] (3) adding iron salt to the acidic solution containing vanadium and arsenic, filtering to obtain ferric arsenate and a high-concentration vanadium-containing acid solution after the reaction, and separating and solidifying the arsenic element in the form of ferric arsenate;

[0082] (4) adding an ammonium source to a high-concentration vanadium-containing acid solution to obtain an acid solution and ammonium polyvanadate after reaction, wherein the acid solution can be reused as an acid dissolving agent.

[0083] Example 1

[0084] This embodiment provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, the method comprising the following steps:

[0085] (1) adding deionized water to dissolve the vanadium arsenic crystals produced when recovering the waste SCR catalyst at a solid-liquid ratio of 1:5, stirring continuously at 80° C. for 3 h, filtering to remove part of the insoluble matter to obtain a high-concentration vanadium arsenic waste liquid, wherein the mass concentration of vanadium element is 14.66 g / L, the mass concentration of arsenic element is 15.61 g / L, the pH value of the vanadium arsenic waste liquid is 13.51, and the volume is 100 mL;

[0086] (2) adding a certain amount of calcium oxide to the vanadium-arsenic waste liquid obtained in step (1), wherein the added amount is added according to a molar ratio of Ca:(V+As) of 5:1 in the solution, stirring at 80° C. for 3 h and filtering to obtain a co-precipitated residue of calcium vanadate and calcium arsenate, washing with deionized water and drying for later use; after testing, the vanadium and arsenic contents in the remaining filtrate are 18.06 mg / L and 23.56 mg / L, respectively, and the pH of the filtrate is 13.9, which can be used as a high-pressure leaching agent for waste SCR catalysts;

[0087] (3) adding 12% by mass sulfuric acid reagent at a solid-liquid ratio of 1:5 to dissolve the calcium vanadate and calcium arsenate residues, stirring at 80° C. for 2 h and filtering, washing with deionized water to obtain a calcium sulfate residue, and the remaining filtrate is a high-concentration vanadium and arsenic solution;

[0088] (4) Add 18 mL of H2O2 solution to the vanadium and arsenic filtrate obtained in step (3), so that the molar amount of H2O2 is 3:1 to the total molar amount of vanadium and arsenic in the vanadium and arsenic filtrate; stir and oxidize at 25°C for 30 minutes to completely convert the arsenic in the solution into pentavalent arsenic; adjust the pH of the solution to 3.0 with 0.5M NaOH solution, then add ferrous sulfate to make the molar ratio of Fe:As in the solution 2.0:1, and react the entire solution in a 30°C water bath for 2 hours. After the reaction is completed, wash and dry the filter residue with deionized water to obtain an iron arsenate precipitate;

[0089] (5) Add ammonium sulfate to the filtrate obtained in step (4) to make NH4 + The molar ratio of vanadium:V is 0.40:1, the pH value of the solution is adjusted to 2.1 with 0.5M H2SO4, and then the solution temperature is heated to 95°C and kept warm for 2 hours. At this time, the vanadium concentration in the supernatant is less than 0.2g / L, and the filtered precipitate is washed with deionized water and dried to obtain the ammonium vanadate product.

[0090] According to calculation, compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic is 98.96%; the recovery rate of vanadium is 92.03%.

[0091] Example 2

[0092] This embodiment provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, the method comprising the following steps:

[0093] (1) adding deionized water to dissolve the vanadium arsenic crystals produced when recovering the waste SCR catalyst at a solid-liquid ratio of 1:7.5, stirring continuously at 85° C. for 2 h, filtering to remove part of the insoluble matter to obtain a high-concentration vanadium arsenic waste liquid, wherein the mass concentration of vanadium element is 10.44 g / L, the mass concentration of arsenic element is 10.87 g / L, the pH value of the vanadium arsenic waste liquid is 13.31, and the volume is 100 mL;

[0094] (2) adding a certain amount of calcium hydroxide to the vanadium-arsenic waste liquid obtained in step (1), wherein the added amount is added according to a molar ratio of Ca:(V+As) in the solution of 4:1, stirring at 80° C. for 3 h and filtering to obtain a co-precipitated residue of calcium vanadate and calcium arsenate, washing with deionized water and drying for later use; after testing, the vanadium and arsenic contents in the remaining filtrate are 25.60 mg / L and 30.29 mg / L, respectively, and the pH of the filtrate is 13.75, which can be used as a high-pressure leaching agent for waste SCR catalysts;

[0095] (3) adding 10% by mass sulfuric acid reagent at a solid-liquid ratio of 1:10 to dissolve the calcium vanadate and calcium arsenate residues, stirring at 80° C. for 2 h and filtering, washing with deionized water to obtain a calcium sulfate residue, and the remaining filtrate is a high-concentration vanadium and arsenic solution;

[0096] (4) Add 10 mL of H2O2 solution to the vanadium and arsenic filtrate obtained in step (3), so that the molar amount of H2O2 is 2:1 to the total molar amount of vanadium and arsenic in the vanadium and arsenic filtrate; stir and oxidize at 25°C for 30 minutes to completely convert the arsenic in the solution into pentavalent arsenic; adjust the pH of the solution to 2.5 with 0.5M NaOH solution, then add ferrous chloride to make the molar ratio of Fe:As in the solution 2.0:1, and react the entire solution in a 40°C water bath for 2.5 hours. After the reaction is completed, wash and dry the filter residue with deionized water to obtain an iron arsenate precipitate;

[0097] (5) Add ammonium chloride to the filtrate obtained in step (4) to make NH4 + The molar ratio of vanadium:V is 0.36:1, the pH of the solution is adjusted to 1.9 with 0.5M H2SO4, and then the solution temperature is heated to 95°C and kept warm for 2 hours. At this time, the vanadium concentration in the supernatant is less than 0.2 g / L, and the precipitate is washed with deionized water and dried to obtain the ammonium vanadate product.

[0098] According to calculation, compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic is 95.36%; the recovery rate of vanadium is 90.26%.

[0099] Example 3

[0100] This embodiment provides a method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, the method comprising the following steps:

[0101] (1) adding deionized water to dissolve the vanadium arsenic crystals produced when recovering the waste SCR catalyst at a solid-liquid ratio of 1:10, stirring continuously at 90° C. for 1.5 h, filtering to remove part of the insoluble matter to obtain a high-concentration vanadium arsenic waste liquid, wherein the mass concentration of vanadium element is 7.345 g / L, the mass concentration of arsenic element is 7.581 g / L, the pH value of the vanadium arsenic waste liquid is 13.18, and the volume is 100 mL;

[0102] (2) adding a certain amount of calcium hydroxide to the vanadium-arsenic waste liquid obtained in step (1), the amount of which is added according to the molar ratio of Ca: (V+As) in the solution of 6:1, stirring at 60° C. for 2 h and filtering to obtain a calcium vanadate and calcium arsenate co-precipitation residue, washing with deionized water and drying for later use; after testing, the vanadium and arsenic contents in the remaining filtrate are 15.05 mg / L and 20.78 mg / L, respectively, and the pH of the filtrate is 13.45, which can be used as a high-pressure leaching agent for waste SCR catalysts;

[0103] (3) adding 13% sulfuric acid reagent at a solid-liquid ratio of 1:15 to dissolve the calcium vanadate and calcium arsenate residues, stirring at 75° C. for 2 h and filtering, washing with deionized water to obtain the calcium sulfate residue, and the remaining filtrate is a high-concentration vanadium and arsenic solution;

[0104] (4) adding 7 mL of H2O2 solution to the vanadium and arsenic filtrate obtained in step (3) so that the molar amount of H2O2 is 2:1 to the total molar amount of vanadium and arsenic in the vanadium and arsenic filtrate; stirring and oxidizing at 25°C for 30 min to completely convert the arsenic in the solution into pentavalent arsenic; adjusting the pH of the solution to 3.0 with 0.5 M NaOH solution, and then adding ferrous sulfate so that the molar ratio of Fe:As in the solution is 3.0:1, and the entire solution is reacted in a 30°C water bath for 2 h. After the reaction is completed, the filter residue is washed and dried with deionized water to obtain an iron arsenate precipitate;

[0105] (5) Add ammonium chloride to the filtrate obtained in step (4) to make NH4 + The molar ratio of vanadium:V is 0.33:1, the pH of the solution is adjusted to 2.3 with 0.5M H2SO4, and then the solution temperature is heated to 95°C and kept warm for 2 hours. At this time, the vanadium concentration in the supernatant is less than 0.2 g / L, and the precipitate is washed with deionized water and dried to obtain the ammonium vanadate product.

[0106] According to calculation, compared with the vanadium-arsenic waste liquid, the precipitation rate of dissolved arsenic is 96.91%; the recovery rate of vanadium is 92.58%.

[0107] Example 4

[0108] The difference between this embodiment and embodiment 1 is that in step (2), the molar ratio of Ca:(V+As) is adjusted to 0.5:1, and the rest is exactly the same as embodiment 1.

[0109] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 83.68% and the recovery rate of vanadium was 78.59%.

[0110] Example 5

[0111] The difference between this embodiment and embodiment 1 is that in step (2), the molar ratio of Ca:(V+As) is adjusted to 6.5:1, and the rest is exactly the same as embodiment 1.

[0112] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 98.20% and the recovery rate of vanadium was 91.51%.

[0113] Example 6

[0114] The difference between this embodiment and embodiment 1 is that in step (4), the molar ratio of Fe:As is adjusted to 0.5:1, and the rest is exactly the same as embodiment 1.

[0115] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 90.28% and the recovery rate of vanadium was 86.95%.

[0116] Example 7

[0117] The difference between this embodiment and embodiment 1 is that in step (4), the molar ratio of Fe:As is adjusted to 3.5:1, and the rest is exactly the same as embodiment 1.

[0118] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 99.17% and the recovery rate of vanadium was 83.29%.

[0119] Example 8

[0120] The difference between this embodiment and embodiment 3 is that in step (4), the oxidation step is omitted, that is, H2O2 solution is not added to the vanadium and arsenic filtrate, but NaOH solution is directly used to adjust the pH value of the vanadium and arsenic filtrate, and the rest is exactly the same as embodiment 3.

[0121] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 80.23% and the recovery rate of vanadium was 75.91%.

[0122] Comparative Example 1

[0123] The difference between this comparative example and Example 1 is that step (2) is omitted, that is, calcium salt is not added to the vanadium-arsenic waste liquid to precipitate vanadium and arsenic; and step (3) is replaced by: using concentrated sulfuric acid with a mass fraction of 12% to adjust the pH value of the vanadium-arsenic waste liquid to 3.0, and the rest is exactly the same as Example 1.

[0124] It was calculated that compared with the vanadium-arsenic waste liquid, the precipitation rate of arsenic was 89.56% and the recovery rate of vanadium was 85.63%.

[0125] Comparative Example 2

[0126] The difference between this comparative example and Example 2 is that step (4) is omitted, that is, H2O2 solution and iron salt are not added to the vanadium and arsenic filtrate, and the step of pre-removing arsenic is not performed. The rest is exactly the same as Example 2.

[0127] It was calculated that the recovery rate of vanadium was 50.23% compared with the vanadium-arsenic waste liquid.

[0128] analyze:

[0129] It can be seen from the results of Examples 1-3 that the method of the present invention can effectively separate vanadium and arsenic, convert arsenic into ferric arsenate precipitation, and recover vanadium in the form of ammonium vanadate product, and the comprehensive recovery rate of vanadium can reach more than 90%. In addition, by adding calcium salt to the vanadium-arsenic waste liquid, vanadium and arsenic can be removed from the high-alkali solution in the form of insoluble calcium vanadate and calcium arsenate, thereby realizing the recovery of the alkali solution. The whole process has a short reaction time, a small overall consumption of reagents, and no waste gas is generated; the amount of wastewater generated is small, and the waste residue is harmless calcium sulfate and ferric arsenate.

[0130] It can be seen from the results of Example 1 and Examples 4-5 that when the molar amount of calcium in the calcium salt is too small to the total molar amount of vanadium and arsenic in the vanadium-arsenic waste liquid, incomplete vanadium-arsenic precipitation will occur and the vanadium recovery rate will be low; when the molar amount of calcium in the calcium salt is too large to the total molar amount of vanadium and arsenic in the vanadium-arsenic waste liquid, the vanadium-arsenic precipitation rate is higher, but it will cause too much calcium ions to be introduced into the alkali solution, affecting the recycling of the alkali solution.

[0131] It can be seen from the results of Example 1 and Examples 6-7 that when the ratio of the molar amount of iron in the iron salt to the molar amount of arsenic in the acidic solution containing vanadium and arsenic is too small, the precipitation rate of arsenic will be low and the precipitation effect of vanadium will be affected; when the ratio of the molar amount of iron in the iron salt to the molar amount of arsenic in the acidic solution containing vanadium and arsenic is too large, the loss rate of vanadium in the solution will be high.

[0132] It can be seen from the results of Examples 3 and 8 that if H2O2 solution is not added in step (4) to oxidize arsenic, the selective recovery rate of vanadium will be greatly reduced.

[0133] It can be seen from the results of Example 1 and Comparative Example 1 that if there is no step of precipitating vanadium and arsenic with calcium salt, irreversible loss of high-concentration alkali solution will result.

[0134] It can be seen from the results of Example 2 and Comparative Example 2 that if the step of adding H2O2 solution and iron salt to remove arsenic in advance is omitted, the selective recovery rate of vanadium will be greatly reduced.

[0135] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid, characterized in that: The method comprises: (1) mixing vanadium-arsenic waste liquid and a precipitant to obtain a precipitate containing vanadium and arsenic after reaction; (2) treating the precipitate containing vanadium and arsenic with acid to obtain an acidic solution containing vanadium and arsenic; (3) mixing the acidic solution containing vanadium and arsenic with an arsenic separation agent, separating arsenic after reaction, and obtaining a vanadium-containing solution; (4) mixing the vanadium-containing solution and an ammonium source to react and obtain the ammonium polyvanadate; The acid used in the acid treatment of step (2) includes a sulfuric acid solution; the mass fraction of the sulfuric acid solution is 8-13%; the ratio of the mass of the precipitate containing vanadium and arsenic to the volume of the sulfuric acid solution is 1g:(5-20)mL; the pH value of the acidic solution containing vanadium and arsenic in step (2) is 1-3; The arsenic separation agent in step (3) comprises an iron salt; the iron salt comprises ferrous chloride and / or ferrous sulfate; the ratio of the molar amount of the iron element in the iron salt to the molar amount of the arsenic element in the acidic solution containing vanadium and arsenic is (1-3):1; In step (3), before the mixing, the acidic solution containing vanadium and arsenic is oxidized, and the pH value of the acidic solution containing vanadium and arsenic after oxidation is adjusted to 2-3.5; the oxidation step specifically includes: mixing the acidic solution containing vanadium and arsenic with an oxidant to carry out an oxidation reaction.

2. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The precipitant in step (1) comprises a calcium salt.

3. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 2, characterized in that: The calcium salt includes at least one of calcium oxide, calcium hydroxide, calcium chloride and calcium sulfate.

4. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 2, characterized in that: The ratio of the molar amount of calcium element in the calcium salt to the total molar amount of vanadium element and arsenic element in the vanadium-arsenic waste liquid is (1-6):

1.

5. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction temperature in step (1) is 25-90°C.

6. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction time of step (1) is 2-3h.

7. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction process of step (1) is accompanied by stirring.

8. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: In step (1), filtering is performed after the reaction to obtain the precipitate and filtrate containing vanadium and arsenic.

9. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 8, characterized in that: The total mass concentration of vanadium and arsenic in the filtrate is 0.5-60 mg / L.

10. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 8, characterized in that: The pH value of the filtrate is 13-14.

11. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The acid treatment method in step (2) specifically comprises: mixing the precipitate containing vanadium and arsenic with an acid and reacting them.

12. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 11, characterized in that: In the acid treatment method, the reaction temperature is 25-80°C.

13. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 11, characterized in that: In the acid treatment method, the reaction time is 2-3 hours.

14. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 11, characterized in that: In the acid treatment method, the reaction process is accompanied by stirring.

15. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The pH value of the oxidized acidic solution containing vanadium and arsenic is adjusted by using alkaline solution.

16. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 15, characterized in that: The alkali solution includes a NaOH solution, and the concentration of the NaOH solution is 0.1-1M.

17. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The oxidant includes H2O2.

18. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 17, characterized in that: The ratio of the molar amount of the H2O2 to the total molar amount of the vanadium element and the arsenic element in the acidic solution containing vanadium and arsenic is (1-4):

1.

19. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The oxidation reaction time is 30-60 minutes.

20. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction temperature in step (3) is 25-40°C.

21. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction time of step (3) is 2-3h.

22. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction process of step (3) is accompanied by stirring.

23. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The ammonium source in step (4) includes an ammonium salt.

24. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 23, characterized in that: The ammonium salt includes ammonium chloride and / or ammonium sulfate.

25. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 23, characterized in that: The ratio of the molar amount of ammonium ions in the ammonium salt to the molar amount of vanadium element in the vanadium-containing solution is (0.33-0.4):

1.

26. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: In step (4), after the vanadium-containing solution and the ammonium source are mixed, the pH value of the obtained mixed solution is adjusted to 1.9-2.

3.

27. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction temperature in step (4) is 80-100°C.

28. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction time of step (4) is 0.5-3h.

29. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The reaction process of step (4) is accompanied by stirring.

30. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: In step (4), filtering is performed after the reaction to obtain the ammonium polyvanadate and a clear liquid.

31. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 30, characterized in that: The concentration of vanadium in the clear solution is less than 0.2 g / L.

32. The method for selectively preparing ammonium polyvanadate from vanadium-arsenic waste liquid according to claim 1, characterized in that: The method specifically comprises: (I) adding calcium salt to vanadium-arsenic waste liquid, reacting at 25-90° C. for 2-3 hours, and filtering to obtain a co-precipitate of calcium vanadate and calcium arsenate and a filtrate, wherein the total mass concentration of vanadium and arsenic in the filtrate is 0.5-60 mg / L; (II) adding a sulfuric acid solution to the calcium vanadate and calcium arsenate coprecipitate, reacting at 25-80° C. for 2-3 hours, and filtering to obtain an acidic solution containing vanadium and arsenic and a calcium sulfate filter residue, wherein the pH value of the acidic solution containing vanadium and arsenic is 1-3; (III) using alkaline solution to adjust the pH value of the acidic solution containing vanadium and arsenic to 2-3.5, then adding H2O2 to the acidic solution containing vanadium and arsenic with adjusted pH value, and performing oxidation reaction for 30-60 minutes, then adding iron salt to the oxidized acidic solution containing vanadium and arsenic, reacting at 25-40°C for 2-3 hours, and then filtering to obtain iron arsenate residue and vanadium-containing solution, wherein the pH value of the vanadium-containing solution is 2-4; (IV) adding an ammonium source to the vanadium-containing solution, adjusting the pH value of the obtained mixed solution to 1.9-2.3, reacting at 80-100° C. for 0.5-3 h, and filtering to obtain the ammonium polyvanadate and a clear solution, wherein the concentration of vanadium in the clear solution is less than 0.2 g / L.

Citation Information

Patent Citations

  • A method for arsenic removal by a tungsten, vanadium, arsenic-containing catalyst

    CN104492421B

  • Methods and applications for separating vanadium, tungsten, and arsenic from sodium hydroxide waste liquid.

    CN112553469B

  • Method for innocent treatment of arsenic-containing waste SCR denitration catalyst

    CN113430381A

  • Method for purifying vanadium pentoxide

    CN104843789A

  • Method for extracting vanadium and removing arsenic from arsenic-containing waste sulfuric acid catalyst

    CN107557584A