Production of Boron Nitride Nanosheets

By using high-viscosity liquid ball milling media and low-impact ball milling technology of polymer materials, combined with ultrasonic vibration, the problems of small size and many defects of boron nitride nanosheets in the existing technology have been solved, and the production of large-sized, high-quality nanosheets has been achieved. Produced for a variety of applications.

CN116457303BActive Publication Date: 2024-10-22DEAKIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180075769.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-21
Filing Date
2021-09-02
Publication Date
2024-10-22
Estimated Expiration
2041-09-02

AI Technical Summary

Technical Problem

Existing ball milling technology is difficult to produce large-sized, high-quality boron nitride nanosheets, and the nanosheets have a large number of defects, which affects their performance in nanocomposites, corrosion protection, and thermal conductivity.

Method used

High-viscosity liquid ball milling media and polymer material ball milling equipment are used to reduce the impact of the ball milling equipment on boron nitride crystals. Boron nitride nanosheets are produced through low-impact peeling technology, and ultrasonic vibration is combined to improve the peeling efficiency and the lateral size of the product. .

Benefits of technology

The size and quality of boron nitride nanosheets are significantly improved, the defect density is reduced, and large-scale production of high-quality nanosheets with high efficiency and low cost is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116457303B_ABST
    Figure CN116457303B_ABST
Patent Text Reader

Abstract

A method for producing boron nitride nanosheets, comprising: grinding a hexagonal boron nitride crystalline material in a ball mill to exfoliate substantially two-dimensional nanosheets from the boron nitride crystalline material, wherein the ball milling is performed in a viscous liquid ball milling medium having a viscosity of 100 to 100,000 mPa·s.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to the production of boron nitride nanosheets (also known as white graphene) from hexagonal boron nitride crystals using ball milling techniques, and the invention will conveniently be disclosed hereinafter in relation to this exemplary application. Background of the Invention

[0003] The following discussion of the background to the invention is intended to facilitate understanding of the invention. However, it should be appreciated that the discussion is not an acknowledgement or admission that any of the material referred to was published, known or part of the common general knowledge as at the priority date of the application.

[0004] Currently, there is a worldwide interest in two-dimensional (2D) nanosheets including graphene, hexagonal boron nitride (hBN), and molybdenum disulfide (MoS 2 There is interest in hBN nanosheets because of their attractive mechanical, thermal and electronic properties. hBN nanosheets have many unique properties such as wide band gap, deep ultraviolet light emission, high thermal conductivity and stability, controllable electrical conductivity and unique wettability. hBN is also considered a green lubricant that can be used in engine oils at high temperatures.

[0005] Similar to other 2D materials, hBN nanosheets (BNNS) can be produced in either a bottom-up or top-down manner. The bottom-up approach includes chemical vapor deposition and segregation methods; the top-down approach is to peel off bulk hBN crystals via mechanical or sonication methods.

[0006] Many studies, such as Deepika et al. High-Efficient Production of Boron Nitride Nanosheets via an Optimized Ball Milling Process for Lubrication in Oil. Sci. Rep. 4, 7288; DOI: 10.1038 / srep07288 (2014), have shown that tailored wet ball milling is an efficient and high-yield method for producing atomically thin BN nanosheets with considerable crystallinity.

[0007] Although tailor-made wet ball milling is the most promising method for producing large quantities of BNNS at a relatively low cost, there are two major problems that have not yet been solved. The first problem is that the size of BNNS produced by existing ball milling methods is small, even when liquid grinding media is included, most of which are between 0.5 and 1.0 μm. The second problem is that the quality of BNNS from ball milling is relatively low, including an unacceptable number of defects.

[0008] These two issues are related to the nature of ball milling technology, which is traditionally designed to introduce high-energy impacts to nanoparticles to break them up. The size and quality of BNNSs are important for improving the properties of this material for many applications, such as stronger nanocomposites, better corrosion protection and superior thermal conductivity.

[0009] Examples of ball milling configurations for producing two-dimensional materials such as graphene or hexagonal boron nitride are taught in Chinese patent publications CN 110203896 A and CN 109956499 A. Each of these patent publications teaches that the use of polymer grinding balls and / or grinding equipment together with secondary (i.e., separate process steps) ultrasound of the grinding material can improve the production of two-dimensional materials. However, these documents do not investigate the optimization of other ball milling parameters for the production characteristics of the two-dimensional material.

[0010] Based on the above, there is still some scope to improve the ball milling production technique for forming boron nitride nanoplatelets. It would therefore be desirable to provide an alternative or improved ball milling method and / or apparatus for producing boron nitride nanoplatelets. Summary of the invention

[0011] A first aspect of the present invention provides a method for preparing boron nitride nanosheets, comprising:

[0012] grinding a hexagonal boron nitride crystalline material in a ball mill to exfoliate substantially two-dimensional nanosheets from the boron nitride crystalline material,

[0013] The ball milling is carried out in a viscous liquid ball milling medium having a viscosity of 100 to 100,000 mPa·s.

[0014] The present invention provides an improved system for producing boron nitride nanosheets (BNNS - also characterized as two-dimensional boron nitride crystalline materials and also referred to as white graphene) by using ball milling media and / or equipment designed to reduce the impact of the ball milling equipment on the feed hexagonal boron nitride crystalline material and the energy thus transferred from the ball milling equipment to the feed hexagonal boron nitride crystalline material compared to conventional methods. The ball mill performs a grinding process, typically a low-impact grinding process, which grinds or peels / peels off essentially two-dimensional nanosheets from the grain surface of the boron nitride crystalline material. Lower impact peeling reduces defects present in the peeled material and can result in larger-sized sheets produced by the method compared to prior art ball milling methods.

[0015] The present invention thus overcomes the problems of previous attempts to produce BNNS by ball milling, namely increasing the size of the BNNS product and minimizing the defects generated during the ball milling process. In order to reduce ball-to-ball and ball-to-jar impact, grinding media with high viscosity are used. As a result, BNNS with diameters an order of magnitude larger and lower defect density than those produced by previous conditions can be produced. However, other factors that affect BNNS production (e.g., grinding ball and grinding equipment material properties as discussed above) have been found, and no correlation has been found before between the viscosity of the grinding and stripping media and the yield, size and quality of the final BNNS product.

[0016] The commercial application of BNNS depends on the large-scale production of high-quality materials with high efficiency and low cost. The present invention provides such a BNNS production route for various applications.

[0017] By the viscosity of the grinding media used in the ball mill, lower impact ball milling is provided in the configuration of the present invention. The traditional wet ball milling equipment for producing BNNS typically uses a liquid medium with low viscosity, which provides the freedom of movement of the grinding balls in the grinding container during the grinding process. However, it is not desired to be limited to any one theory, and the inventors have found that the viscosity of the grinding media, rather than its chemical composition, is important for the impact control during the stripping process. The inventors have found that the highly viscous wet media can be used to reduce the impact of the grinding balls during the grinding by helping to slow down the movement, and therefore reduce the energy transfer during the impact between the grinding balls and the material (boron nitride crystal) ground during the grinding.

[0018] The viscous liquid milling media has a viscosity of 100 to 100,000 mPa·s. In some embodiments, the viscous liquid milling media has a viscosity of 200 to 50000 mPa·s, preferably 500 to 20000 mPa·s, more preferably 1000 to 20000 mPa·s and still more preferably 1000 to 10000 mPa·s.

[0019] It will be appreciated that the viscosity of the liquid medium of the present invention is measured by a rheometer of the type using an oscillating test (shear rheometer). An illustrative example of a suitable rheometer is the HR-3, TA Instruments, USA.

[0020] A variety of different compositions, including those listed below, may be used to produce the appropriate viscosity of the grinding media. However, it should be understood that the present invention is not limited to those specific compositions and will extend to other compositions and grinding media not specifically listed.

[0021] These novel viscous liquid milling media of the present invention that can be used have three general groups selected from at least one of the following:

[0022] i. High viscosity liquid;

[0023] ii. using a high viscosity solution of a high molecular weight organic solute dissolved in a solvent; or

[0024] iii. Materials that are melted to form molten grinding media.

[0025] First, a material in liquid form and with high viscosity, such as a slurry, such as a slurry based on sugar or polyethylene glycol. In some forms, the syrup can be a slurry solution based on sucrose. Each of these materials has a relatively low molecular weight. Note that sugar / sucrose is in a viscous liquid form in this embodiment.

[0026] The term sugar in this specification refers to pure carbohydrates, such as sugars, more particularly monosaccharides and disaccharides. The grinding media of the present invention may contain any suitable sugar-based solution or syrup that provides the required liquid viscosity. Examples of suitable sugars include monosaccharides such as glucose, fructose and galactose; disaccharides such as sucrose, lactose or maltose or combinations thereof. In some embodiments, the syrup may be based on ordinary sugar consisting essentially of sucrose.

[0027] In certain embodiments, the sugar content of the syrup-based grinding media composition comprises an aqueous sugar solution comprising a 50-90% w / w solution, preferably a 50-80% w / w sugar solution, more preferably a 60-75% w / w solution. Such a sugar solution may be formed in some embodiments by dissolving sugar (e.g., domestic grade raw sugar) in hot water or other suitable solvent. However, various other sugar solution / syrup preparation methods may also be used.

[0028] Secondly, wherein the high viscosity solution comprises polyvinyl alcohol or polyacrylamide dissolved in water, ethanol or another suitable solvent. In this respect, there is a material (mostly organic materials) with high solubility in water, ethanol or other solvents that form a high viscosity solution. Examples include polyvinyl alcohol or polyacrylamide, each of which has a very large molecular weight.

[0029] It should be appreciated that the inclusion of an organic medium can also add functional groups to the surface of the BNNS, with the advantage of being less likely to agglomerate and more easily integrated with polymer composites.

[0030] Third, the molten grinding media comprises molten polymers. In this regard, molten materials such as molten polymers can be used when heated to a temperature greater than their melting temperature. An example is a polyurethane in a molten phase at >60°C. Polyurethane can go from a solid at room temperature to a molten phase at >60°C, thereby providing a grinding media with a high viscosity.

[0031] The grinding media is preferably removable by washing with water, ethanol and other solvents, more preferably easily removable by washing with water, ethanol and other solvents. For example, when syrup is used, the grinding media can be easily removed using water.

[0032] It is preferred that the grinding media is compatible with the grinding ball and grinding container material. For example, when the grinding ball and grinding container material comprises a polymeric material such as nylon, polyethylene, acetal or polystyrene, it is preferred that the grinding media is selected to be compatible with the material.

[0033] The temperature of the grinding media can be controlled to change the viscosity of the grinding media. The method of the first aspect can therefore also include controlling the temperature of the grinding media during ball milling to provide the desired viscosity during ball milling. For example, a lower temperature can be used to improve the viscosity of a polymer solution such as a polyvinyl alcohol ethanol solution. Another example is to use an elevated temperature to melt the polymer to form a high viscosity grinding media. In contrast, all previous special wet ball milling methods for producing BNNS are carried out at room temperature without the need to use any temperature control.

[0034] In some embodiments, ball milling with lower impact on the configuration of the present invention can also be improved by selecting materials for the ball milling container and grinding balls. Conventional ball milling equipment for producing boron nitride nanosheets typically uses metal or ceramic ball milling jars and balls, which can significantly reduce the size of the BNNS product and produce a large number of defects in them. In the present invention, one or both of the grinding balls and the grinding container may preferably be composed of a polymer material. Examples of suitable polymer materials include plastics such as nylon, polyethylene, acetal or polystyrene; or rubber. The density of these polymer materials is much lower than that of ceramics or metals and therefore produces lower impact on bulk boron nitride crystals during grinding. This can maximize the size and quality of the BNNS product. In addition, the use of lighter grinding jars and balls can be more cost-effective than metal or ceramic equivalents because this can result in considerable energy savings during operation.

[0035] The grinding parameters including grinding speed, grinding time, ball to powder ratio and grinding ball size can be varied for a particular ball mill configuration to optimize exfoliation efficiency and production yield. It should be understood that these parameters are highly dependent on the type and size of the grinding apparatus and grinding vessel, the material, density, size and number of grinding balls and the viscosity of the grinding media.

[0036] Examples of parameters in specific embodiments include a ball mill rotation speed of 50 to 300 rpm, preferably 50 to 200 rpm. In some embodiments, the ball milling temperature is room temperature to 150° C., preferably 20° C. to 80° C. In some embodiments, the ball milling is performed for a grinding time of 1 to 200 hours, preferably 1 to 100 hours.

[0037] Furthermore, grinding balls with diameters of 0.1 to 5.0 mm in many embodiments can effectively exfoliate BN particles into BNNS.

[0038] Ball milling can be performed at multiple conductions. In some embodiments, ball milling is performed in an air atmosphere or an inert atmosphere mixture. In embodiments, the inert atmosphere can be a nitrogen atmosphere, an argon atmosphere, or a helium atmosphere.

[0039] The feed material for grinding / stripping in the ball mill is a hexagonal boron nitride crystal (hBN) material. The feed hBN material is typically formed into flat disc-shaped or plate-shaped particles with a thickness of tens, hundreds or thousands of nanometers. Depending on the source of hBN, the feed material may have various properties. In some embodiments, the starting hBN particles have a typical disc-shaped shape with a diameter (average diameter / size in a flat plane) of 0.5 to 100 μm, preferably 5-80 μm and more preferably 10-50 μm. In an embodiment, the thickness of the feed hBN is on the order of 50 to 500 nm, preferably 50 to 200 nm and about 100 nm in some embodiments.

[0040] Ball milling according to the present invention can be combined with ultrasound in some embodiments to enhance the exfoliation of two-dimensional boron nitride nanosheets from bulk crystals. Ball milling and ultrasound use different mechanisms to exfoliate BNNS, and the combination of the two techniques can greatly improve the efficiency and yield of the process. In such an embodiment, the method may also include the following steps:

[0041] Ultrasonic vibrations are applied to the viscous milling media during milling.

[0042] Adding ultrasound / ultrasound to the milling process can help the exfoliation of hexagonal boron nitride (hBN). Compared with traditional ball milling alone, the addition of ultrasound has greater productivity and helps produce BNNS with larger lateral dimensions.

[0043] Ultrasonic vibrations may be applied to the viscous milling media before, during or after the ball milling operation. In a preferred embodiment, ultrasonic vibrations are applied to the viscous milling media during the ball milling operation. In some embodiments, the ultrasonic vibrations have a frequency of 18 to 200 kHz, preferably 18 to 180 kHz, more preferably 18 to 150 kHz. In an embodiment, the ultrasonic vibrations have a frequency of 20 to 180 kHz, preferably 50 to 150 kHz. In one embodiment, the ultrasonic component has a frequency of 40 kHz and a power of 300 W.

[0044] The present invention is applicable to various ball mill configurations. In some embodiments, the ball mill comprises at least one of the following: a conventional ball mill, a planetary ball mill, or a stirred ball mill.

[0045] A second aspect of the present invention provides an apparatus for producing boron nitride nanosheets, comprising:

[0046] a ball mill comprising a plurality of grinding balls and a container configured to receive and surround the hexagonal boron nitride crystalline particles, the plurality of grinding balls, and a liquid milling medium, the ball mill being configured to drive movement of the grinding balls within the container and thereby exfoliate substantially two-dimensional nanosheets from the hexagonal boron nitride crystalline material when immersed in the liquid milling medium;

[0047] The liquid milling medium comprises a viscous liquid having a viscosity of 100 to 100000 mPa·s.

[0048] As outlined above, the operation of the ball mill drives the movement of the grinding balls within the container, thereby causing the grinding balls to apply a combination of impact, friction and shear forces to the boron nitride crystalline material, and thereby exfoliate the boron nitride crystalline material into substantially two-dimensional nanosheets. This grinding process grinds, shears or exfoliates substantially two-dimensional nanosheets from the crystal surface of the boron nitride crystalline material. The ball mill efficiently exfoliates hexagonal boron nitride (hBN) particles into atomically thin BNNS while generating minimal in-plane defects.

[0049] The viscous liquid milling media has a viscosity of 100 to 100000 mPa·s. In some embodiments, the viscous liquid milling media has a viscosity of 200 to 50000 mPa·s, preferably 500 to 20000 mPa·s, more preferably 1000 to 20000 mPa·s and still more preferably 1000 to 10000 mPa·s.

[0050] Again, the viscous liquid milling medium preferably comprises at least one of the following:

[0051] High viscosity liquid;

[0052] Use a high viscosity solution of a high molecular weight organic solute dissolved in a solvent; or

[0053] The material is melted to form the molten grinding media.

[0054] It should be understood that the above three aspects are similar to those taught in relation to the first aspect. This disclosure is equally applicable to this second aspect of the invention.

[0055] To further control or select the viscosity of the grinding media, the apparatus may also include a temperature controller configured to control the temperature of the grinding media during ball milling to provide a desired viscosity during ball milling.

[0056] In some embodiments, the ball mill comprises at least one of ball milling balls or a ball milling container comprising a polymer material. The polymer material of the ball milling balls or the ball milling container may comprise any suitable polymer material. In an embodiment, the polymer material may comprise at least one of the following: plastic or rubber, preferably nylon, polyethylene, acetal and polystyrene.

[0057] Any suitable ball milling configuration may be used with the present invention.In many embodiments, the ball mill comprises at least one of: a conventional ball mill, a planetary ball mill, or an agitator ball mill.

[0058] As in the first aspect, the apparatus may further comprise a high frequency ultrasonic transducer operably connected to the liquid grinding medium and capable of applying at least 18 to 200 kHz ultrasonic frequencies to the liquid grinding medium during operation of the ball mill. In some embodiments, the ultrasonic vibration has a frequency of 18 to 200 kHz, preferably 18 to 180 kHz, and more preferably 18 to 150 kHz.

[0059] Any suitable configuration may be used to add ultrasonic frequencies / vibrations to the device. In a first embodiment, a sheath comprising an ultrasonic transducer is added to the outside of the ball milling container. In other embodiments, an ultrasonic transducer / generator is added to the inside or one or more walls of the ball milling container.

[0060] A third aspect of the invention provides boron nitride nanosheets (BNNS) produced according to the method of the first aspect of the invention. In embodiments, these BNNS have an average particle size of 5 to 10 μm. Most of the BNNS from the previous ball milling method have a diameter of 0.5 to 1.0 μm. BNNS formed using the method and apparatus of the present invention can therefore be produced one order of magnitude larger than those that can be produced using conventional ball milling materials and grinding media. In addition, BNNS produced using the method and apparatus of the present invention can show less damage to their structure compared to BNNS produced using prior art ball milling methods and configurations. The product preferably comprises atomically thin BNNS that typically have minimal in-plane defects.

[0061] BRIEF DESCRIPTION OF THE DRAWINGS

[0062] The invention will now be described with reference to the figures of the accompanying drawings, which illustrate particularly preferred embodiments of the invention, in which:

[0063] Figure 1 is a schematic diagram of a conventional ball milling apparatus constructed in accordance with one embodiment of the present invention.

[0064] Figure 2 is a schematic diagram of a planetary ball milling apparatus constructed according to one embodiment of the present invention.

[0065] Figure 3 Provided are SEM images of the hexagonal boron nitride starting material utilized in the ball milling experimental runs.

[0066] Figure 4A , 4B4C and 4C provide SEM images of the product hexagonal boron nitride material after ball milling in syrup milling media and using acetal (plastic) milling balls using a method according to one embodiment of the present invention.

[0067] Figure 5A , 5B 5C and 5C provide SEM images of the product hexagonal boron nitride material after ball milling in aqueous milling media and using acetal (plastic) milling balls using a method according to one embodiment of the present invention.

[0068] Fig. 6A , 6B 6C and 6C provide SEM images of the product hexagonal boron nitride material after ball milling in syrup milling media and using steel milling balls using a method according to one embodiment of the present invention.

[0069] Fig. 7A , 7B 7C and 7C provide SEM images of the product hexagonal boron nitride material after ball milling in aqueous milling media and using steel milling balls according to the first comparative / control ball milling method.

[0070] Fig. 8A , 8B 8C and 8C provide SEM images of the product hexagonal boron nitride material after ball milling in solid sugar grinding media and using steel grinding balls according to a second comparative / control ball milling method.

[0071] Details

[0072] Boron nitride nanosheets (BNNS), also known as white graphene, have many fascinating properties. The present invention relates to a method for producing BNNS using a ball milling device under special conditions, which efficiently exfoliates hexagonal boron nitride (hBN) particles into large-sized atomically thin BNNS while generating minimal in-plane defects. The production method of the present invention can potentially be expanded to facilitate large-scale production of BNNS.

[0073] Conventional ball milling of hexagonal BN, such as horizontal or vertical ball milling, has the advantage of being a simple method and has the potential for large-scale production of BNNS. However, ball milling not only applies shear forces that produce peeling effects, but they also generate considerable impact forces due to the collision of the balls. The impact forces reduce the lateral size of the BNNS and also adversely affect their lattice structure. Therefore, BNNS prepared by this method usually have small lateral sizes and a large number of lattice defects.

[0074] Conventional ball milling equipment for producing BNNS typically uses metal or ceramic milling jars and balls, which greatly reduce the size of the BNNS products and create a large number of defects in them. Conventional wet ball milling equipment for producing boron nitride nanosheets typically uses a liquid medium with low viscosity, thereby deteriorating the size and quality of the BNNS products.

[0075] The inventors unexpectedly discovered that careful selection of ball milling media can reduce the impact of the ball milling equipment on the boron nitride crystalline material and the energy thus transferred from the ball milling equipment to the boron nitride crystalline material compared to the traditional ball milling method. Lower impact peeling reduces the defects present in the peeled material and can lead to larger-sized sheets produced by this method. The peeling of hBN particles into BNNS is a process of overcoming the van der Waals interlayer interactions, which has very low energy (about 10meV / unit cell). In contrast, normal ball milling impact has high energy, up to 5 orders of magnitude higher than that required to peel hBN or overcome its interlayer interactions. The much larger ball milling impact energy destroys the in-plane structure of BNNS, resulting in smaller lateral sizes and relatively high density defects.

[0076] It should be understood that a ball mill is a type of grinding machine used for grinding, blending and sometimes mixing materials. It works on the principle of impact and friction: size reduction is achieved by the impact of the balls as they fall from near the top of the housing. A ball mill consists of a grinding container - typically a hollow cylindrical housing that rotates about its axis. In a non-agitated ball mill, the axis of the housing may be either horizontal or at a small angle to the horizontal. It is partially filled with grinding balls. The grinding media are balls that may be immersed in the grinding media, which covers the grinding balls and feed material in the ball mill. The inner surface of the cylindrical housing may be lined with a wear-resistant material such as manganese steel or a rubber lining. A ball mill operates by the movement of the grinding balls within the grinding container.

[0077] The present invention can be applied to various ball mill configurations. In some embodiments, the ball mill comprises at least one of the following: a conventional ball mill, a planetary ball mill, or a stirred ball mill. Figure 1 and 2 2 illustrates two examples of ball milling configurations that can be used to produce BNNS according to the method and apparatus of the present invention. It should be understood that other ball milling configurations may also be suitable for the present invention, and the present invention should not be limited to the ball milling configurations illustrated in the drawings.

[0078] Figure 11. A conventional ball mill 100 is illustrated in FIG. Such a ball mill 100 comprises a grinding vessel in the form of a cylindrical housing 105 oriented horizontally and longitudinally. The housing 105 houses a plurality of grinding balls 110, feed material / particles 120 (hBN material) to be ground, all immersed in a liquid grinding medium 130. As the housing 105 rotates in a direction R, the grinding balls 100 are lifted on the rising side of the housing 105 and then they fall (or drop onto the feed material 120) from near the top of the housing 105. In doing so, the solid feed particles 120 between the grinding balls 110 and between the balls 110 and the housing 105 experience impact and shear forces thereon.

[0079] Planetary ball mill 100A( Figure 2 ) consists of at least one grinding container in the form of a grinding jar 105A arranged eccentrically on a sun wheel or planetary disk 140. The planetary disk 140 is driven to rotate in a rotation direction D opposite to the rotation direction R of the grinding jar 105A, usually with a ratio of 1:-2 or 1:-1. The grinding balls 110 are contained in the grinding jar 105 together with the feed material / particles 120 to be ground (in this case hBN material), all immersed in the liquid grinding medium 130. Due to the Coriolis force, the grinding balls 110 experience a superimposed rotational motion. The speed difference between the grinding balls 120 and the grinding jar 105A produces an interaction between friction and impact forces, which increases high kinetic energy. The mutual influence between these forces produces high and very effective shear forces on the feed material / particles 120 therein.

[0080] Agitator ball mills (not illustrated) include a rotor or agitator designed to move balls within a housing. In some embodiments, the housing of the agitator ball mill is cylindrical and oriented vertically and longitudinally, with the rotor / agitator positioned around or near the axis of the cylindrical housing.

[0081] In each of these embodiments, the conventional ball milling configuration has been modified to use a liquid milling medium 130 comprising a viscous liquid having a viscosity of 100 to 100,000 mPa·s. In addition, at least one of the milling balls 110 or the containers 105, 105A may also comprise a polymer material.

[0082] In operation, the ball mill 100, 100A drives the movement of the grinding balls 110 within the container 105, 105A to exert shear forces on the hBN feed material 120 and thereby peel off substantially two-dimensional nanosheets from the crystalline surface of the boron nitride crystalline material 120 when immersed in the liquid ball milling medium 130. The product comprises atomically thin BNNS that typically have large size and minimal in-plane defects. The present invention thus overcomes the problems of previous attempts to produce BNNS by ball milling, namely increasing the size of the BNNS product and minimizing the defects generated during the ball milling process. In order to reduce ball-to-ball and ball-to-jar impacts, grinding media with high viscosity are used. This can be combined with lower density polymer-based grinding balls. As a result, BNNS with a diameter one order of magnitude larger and a lower defect density than those produced by previous conditions can be produced.

[0083] As previously described, the polymer material of the ball milling balls 110 or the ball milling containers 105, 105A may comprise any suitable polymer material. In an embodiment, the polymer material may comprise at least one of the following: plastic or rubber, preferably nylon, polyethylene, acetal, and polystyrene. In addition, the viscous liquid ball milling media 130 preferably comprises at least one of the following: a high viscosity liquid, a high viscosity solution using a high molecular weight organic solute dissolved in a solvent, or a material that melts to form a molten grinding medium.

[0084] To further control or select the viscosity of the grinding media, the ball mill 100, 100A may also include a temperature controller (not illustrated) configured to control the temperature of the grinding media during ball milling to provide a desired viscosity during ball milling.

[0085] Further processing using ultrasound can be used to further delaminate hBN powder into BNNS. This type of ultrasonic method (which is widely used to exfoliate graphite in the manufacture of graphene) has the advantage of being a simple method and exerting a negligible effect on the lattice structure of BNNS. However, the difference in electronegativity between B and N atoms in adjacent hBN layers leads to an increase in interlayer interactions (i.e., edge-edge (lip-lip) interactions) other than weak van der Waals forces, resulting in a more difficult exfoliation process for hBN than when the method is applied to graphite. Therefore, the BNNS yield of the ultrasonic exfoliation method alone can be very low, and the lateral size of the obtained BNNS decreases accordingly with the increase of the ultrasonic time. The combination of the ball milling method and instrument of the present invention with ultrasound provides an enhanced exfoliation method, which helps and / or enhances the exfoliation of hexagonal boron nitride (hBN) produced during or by ball milling. Compared with conventional ball milling alone, the addition of an ultrasonic method has greater productivity and helps produce BNNS with larger lateral sizes.

[0086] Any suitable configuration (not illustrated) may be used to add ultrasonic frequencies to the device. In a first embodiment, a sheath comprising an ultrasonic transducer is added to the outside of the grinding container. In other embodiments, an ultrasonic transducer / generator is added to the inside of the ball mill container or to one or more walls.

[0087] Ultrasonic vibrations may be applied to the viscous milling media before, during or after the ball milling operation. In a preferred embodiment, ultrasonic vibrations are applied to the viscous milling media during the ball milling operation. In some embodiments, the ultrasonic vibrations have a frequency of 18 to 200 kHz, preferably 18 to 180 kHz, more preferably 18 to 150 kHz. In one embodiment, the ultrasonic component has a frequency of 40 kHz and a power of 300 W. Example

[0088] It should be understood that in the following examples, the viscosity of the grinding media, rather than its chemical composition, is important for impact control during the stripping process. A variety of different compositions can be used to produce the appropriate viscosity of the grinding media. Syrup solutions are used as examples of producing appropriate viscosities. It should be understood that other liquid compositions can be equally used to produce grinding media with similar viscosities. This example is therefore considered to illustrate that grinding media of various compositions are suitable for the grinding method of the present invention.

[0089] Furthermore, although the examples use a planetary mill, it should be understood that the results are equally applicable to other types of ball mills, including traditional / conventional ball mills and agitator ball mills.A planetary mill has been used in the examples for illustrative purposes only.

[0090] experiment

[0091] The production of boron nitride nanoplatelets (BNNS) was carried out in a planetary ball mill (MSE Supplies LLC, USA) under different conditions to show the influence of the materials of the balls and the grinding media.

[0092] The first experimental run was conducted under conditions in accordance with an embodiment of the present invention. In this experimental run, 10 g of hexagonal boron nitride (hBN) particles (Momentive, USA - illustrative particles shown in Figure 3In a zirconium oxide grinding jar, about 200 g of acetal grinding balls with a diameter of 4 mm and 150 mL of a sugar-based syrup (Australian Woolworths flavored maple syrup - having the listed ingredients of sugar (based on sucrose), maltodextrin, dextrose, caramel powder (based on sucrose), water, salt (0.11% w / w), natural flavoring, preservative (202), citric acid) were placed. This sugar-based syrup had a total sugar content of 50% w / w (50 g / 100 g) and a viscosity of 2600 mPa·s, as measured using a HR-3 rheometer (TA Instruments, USA) at 20° C. The grinding speed was 150 rpm and the total grinding time was 5 hours, wherein the direction of rotation was reversed every 1 hour. The grinding atmosphere was air. After the ball milling process, a small amount of sample was taken out of the jar and diluted with water. The solution was sonicated for a short time of 2 minutes. The solution was allowed to stand for 1 hour before taking a drop of the top solution for SEM imaging.

[0093] Two additional experimental runs were also used to produce BNNS to investigate the effects of acetal spheres and slurry solutions on the performance of BNNS produced using the same starting material - hexagonal boron nitride (hBN) particles (Momentive, USA - illustrative particles are shown in Figure 3 The results of the present invention are to investigate the effect of ball milling of BNNS produced by BNNS in the first experiment (in the second experiment). These runs contained: (i) acetal balls in water grinding medium (same as the first experiment); and (ii) steel balls with a diameter of 4 mm in slurry grinding medium following the same procedure as above. The total weight of the steel balls was kept the same as the acetal balls in the first experimental run (about 200 g). The other ball milling conditions were the same for both controls, i.e., the speed was 150 rpm, the milling time was 5 hours, and the milling atmosphere was air.

[0094] Both control runs also used the same starting material - hexagonal boron nitride (hBN) particles (Momentive, USA - illustrative particles are shown at Figure 3 The control 1 used steel balls with a diameter of 4 mm, and the total weight of the steel balls remained the same as the first experimental run (about 200 g); and the grinding medium was water. The control 2 used steel balls with a diameter of 4 mm, and the total weight of the steel balls remained the same as the first experimental run (about 200 g); and the grinding medium was 50 g of solid sugar (Australian CSR white sugar). For both controls, the other ball milling conditions were the same as the first experimental run, i.e., the speed was 150 rpm, the grinding time was 5 hours, and the grinding atmosphere was air.

[0095] result

[0096] The starting hBN particles have a typical disk-like shape with a diameter of 10 to 50 μm and a thickness on the order of 100 nm, as shown by Figure 3 The scanning electron microscopy (SEM) images are shown in Figure 2.

[0097] Results Figure 4A , 4B The BNNS produced by the experimental run of the present invention using plastic (acetal) balls and high viscosity (slurry) grinding media are shown in the SEM images of 4C and 4D. 7A to 8C The control experimental run shown in has much larger size. In addition, the BNNBs produced by the experimental runs of the present invention appear thinner than the BNNS from the two control conditions.

[0098] All previous ball milling methods, as exemplified by control experimental runs (e.g. 7A to 8C The results of these experimental runs confirmed that BNNS from low-density balls and high-viscosity grinding media can produce BNNS with diameters of 5 to 10 μm (see Figure 4A , 4B and 4C, which exhibit particle sizes of 5.3 μm, 7.0 μm, and 7.3 μm, respectively), an order of magnitude larger than those that can be produced using conventional ball milling materials and grinding media.

[0099] When using acetal balls and water grinding media (such as FIG. 5A to FIG. 5C The average size of BNNS was 1.0 to 2.0 μm in diameter when using steel ball and slurry grinding media (as shown in the SEM image of FIG. 6A to FIG. 6C The average size of the BNNS was 2.0 to 3.0 μm when the BNNS was prepared by grinding the BNNS with a light density of 1.2 μm and a viscous grinding medium.

[0100] In addition, when using steel balls and water grinding media (such as 7A to 8C The production yield of thin BNNSs appears to be much lower than that from plastic balls and slurry milling media (as shown in the SEM images of ). This may be due to the smaller number of steel balls used in these ball milling processes. The size of BNNSs from steel balls in water is mainly 0.5 to 1.0 μm ( Figures 7A to 7C ), which is consistent with previous studies such as Deepika et al. High-Efficient Production of Boron Nitride Nanosheets via an Optimized Ball Milling Process for Lubrication in Oil. Sci. Rep. 4, 7288; DOI: 10.1038 / srep07288 (2014). The use of solid sugar and steel balls resulted in even smaller BNNSs, mainly around 0.5 μm ( Figures 8A to 8C ).

[0101] Finally, BNNS ( Figures 7A to 7C ) and the BNNS produced by the experimental operation of the present invention ( Figure 4A , 4B 4C) show greater damage to their structure and thus greater defect levels. During SEM characterization, many highly deformed and wrinkled hBN particles (but not exfoliated into BNNS) could be observed from the samples produced by steel balls compared to the BNNS produced by the experimental runs of the present invention.

[0102] Those skilled in the art will appreciate that the invention described herein is susceptible to changes and modifications other than those specifically described. It is to be understood that the invention includes all such changes and modifications that fall within the spirit and scope of the invention.

[0103] When the terms "comprises", "including", "comprising" or "containing" are used in this specification (including the claims), they should be interpreted as specifying the presence of stated features, integers, steps or components, but not excluding the presence of one or more other features, integers, steps, components or groups thereof.

Claims

1. A method for producing boron nitride nanosheets, wherein include: grinding a hexagonal boron nitride crystalline material in a ball mill to exfoliate substantially two-dimensional nanosheets from the boron nitride crystalline material, The ball milling is carried out in a viscous liquid ball milling medium having a viscosity of 100 to 100,000 mPa·s. 2 . The method according to claim 1 , wherein the viscous liquid milling medium has a viscosity of 200 to 50,000 mPa·s.

3. The method of claim 1, wherein the viscous liquid milling medium comprises at least one of: (i) High viscosity liquid; (ii) using a high viscosity solution of a high molecular weight organic solute dissolved in a solvent; or (iii) Material that is melted to form the molten grinding media. The method of claim 3 , wherein the high viscosity liquid comprises a slurry.

5. The method of claim 4, wherein the high viscosity liquid comprises syrup.

6. The method of claim 3, wherein the high viscosity solution comprises polyvinyl alcohol or polyacrylamide dissolved in water or ethanol.

7. The method of claim 3, wherein the molten grinding media comprises a molten polymer.

8. The method of claim 7, wherein the molten grinding media comprises a polyurethane in a molten phase at >60°C.

9. The method of claim 1, further comprising controlling the temperature of the milling media during ball milling to provide a desired viscosity during ball milling.

10. The method of claim 1, wherein the ball milling is performed using at least one of ball milling balls or ball milling containers comprising a polymer material.

11. The method of claim 10, wherein the polymer material of the milling balls or milling containers comprises at least one of: plastic or rubber.

12. The method of claim 1, wherein the ball mill comprises at least one of the following: a conventional ball mill, a planetary ball mill, or an agitator ball mill.

13. The method according to claim 1, further comprising: The following steps are involved: Ultrasonic vibrations are applied to the viscous liquid milling media during milling.

14. The method of claim 13, wherein the ultrasonic vibration has a frequency of 18 to 200 kHz.

15. The method according to claim 1, wherein the ball milling is performed in an air atmosphere or an inert atmosphere mixture.

16. A system for producing boron nitride nanosheets, comprising: (i) a ball mill comprising a plurality of grinding balls and a container configured to receive and surround the hexagonal boron nitride crystalline material and the plurality of grinding balls, and (ii) a liquid milling medium in the ball mill, the liquid milling medium comprising a viscous liquid having a viscosity of 100 to 100,000 mPa·s, wherein the ball mill is configured to drive the movement of the grinding balls within the container and thereby exfoliate substantially two-dimensional nanosheets from the hexagonal boron nitride crystalline material when the hexagonal boron nitride crystalline material is immersed in the liquid milling medium within the ball mill.

17. The system of claim 16, wherein the liquid milling medium has a viscosity of 200 to 50,000 mPa·s.

18. The system of claim 16, wherein the liquid milling medium comprises at least one of: (i) High viscosity liquid; (ii) using a high viscosity solution of a high molecular weight organic solute dissolved in a solvent; or (iii) Material that is melted to form the molten grinding media.

19. The system of claim 18, wherein the high viscosity liquid comprises a slurry.

20. The system of claim 18, wherein the high viscosity solution comprises polyvinyl alcohol or polyacrylamide dissolved in water or ethanol.

21. The system of claim 18, wherein the molten grinding media comprises a molten polymer.

22. The system of claim 16, wherein the ball mill comprises at least one of milling balls or a milling container comprising a polymer material.

23. The system of claim 22, wherein the polymer material of the milling balls or milling containers comprises at least one of: plastic or rubber.

24. The system of claim 16, further comprising a temperature controller configured to control the temperature of the ball milling media during ball milling to provide a desired viscosity during ball milling.

25. The system of claim 16, wherein the ball mill comprises at least one of: a conventional ball mill, a planetary ball mill, or an agitator ball mill.

26. The system of claim 16, further comprising a high frequency ultrasonic transducer operably connected to the liquid milling medium and capable of applying an ultrasonic frequency of 18 to 200 kHz to the liquid milling medium during operation of the ball mill.

27. Boron nitride nanosheets produced by the method according to any one of claims 1 to 15.

28. The boron nitride nanosheets according to claim 27, having an average particle size of 1 to 10 µm.