Asphalt modified cement-based composite material and preparation method and application thereof
Through the combination of graphene oxide modified cement and emulsified asphalt, an asphalt-modified cement-based composite material is formed, which solves the problems of low strength and insufficient toughness of traditional cement-emulsified asphalt composite materials, and significantly improves the mechanical properties and solidification of oil well cement sheaths. Well quality.
Patent Information
- Application Number
- CN202310437220.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Traditional cement-emulsified asphalt composite materials have low early strength, slow strength formation process, difficult to control the demulsification speed of emulsified asphalt, and limited toughening effect, resulting in insufficient mechanical properties of the oil well cement sheath, affecting cementing quality and safety.
Graphene oxide is used to modify cement, and is mixed with emulsified asphalt and defoaming agent. Asphalt-modified cement-based composite materials are prepared through ultrasonic and surfactant treatment to form a more complete spatial network structure and improve strength and toughness.
It significantly improves the early strength and toughness of the cement sheath, extends the life of the mechanical properties, and enhances the cementing quality and safety.
Smart Images

Figure BDA0004192675540000071
Abstract
Description
Technical Field
[0001] The invention relates to an asphalt-modified cement-based composite material and a preparation method and application thereof, belonging to the technical field of oil well cement-based composite materials. Background Art
[0002] During the oil and gas production process, the quality of cementing directly affects the safe production life of oil and gas wells and the efficiency of oil and gas production. Among them, the quality of cementing mainly depends on the mechanical strength of the cement sheath. The cement sheath refers to the cement stone formed by cement slurry in the annular space. Its function is to wrap the casing hoop into a ring. After the cementing operation, the casing and the formation are bonded together by the cement sheath (that is, cement stone). The cement sheath is made of special cement (that is, oil well cement). Under the coupling effect of downhole working conditions and high temperature and high pressure at the bottom of the well, the mechanical strength and interlayer sealing ability of the cement sheath gradually decline, eventually leading to annular channeling, and even causing huge economic losses and endangering the lives of construction workers. Therefore, high requirements are placed on the mechanical properties of the cement sheath.
[0003] Cement sheath is a typical brittle material. Improving the toughness of oil well cement is the key to improving the cementing quality of oil and gas wells. Emulsified asphalt is a liquid asphalt of water-in-oil or oil-in-water generated by asphalt and emulsifier under certain process. It has low viscosity and excellent fluidity. It can be used at room temperature and can also be used with cold and wet stones. It is an environmentally friendly and low-carbon emission material. Studies have shown that using asphalt materials with viscoelastic properties to modify cement is a feasible solution to effectively improve the toughness of cement matrix. This organic-inorganic composite system takes into account the advantages of cement materials and asphalt materials, and has certain strength, toughness and deformation capacity. However, traditional cement-emulsified asphalt composite materials have defects such as low early strength, slow strength formation process, difficult to control the demulsification rate of emulsified asphalt, and limited toughening effect. Summary of the invention
[0004] The purpose of the present invention is to provide an asphalt-modified cement-based composite material and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.
[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0006] One aspect of the present invention provides a method for preparing an asphalt-modified cement-based composite material, comprising:
[0007] Modifying cement with graphene oxide to obtain graphene oxide modified cement;
[0008] The emulsified asphalt, the defoamer and the graphene oxide modified cement are evenly mixed to prepare an asphalt modified cement-based composite material.
[0009] In the present invention, the preparation method of the asphalt-modified cement-based composite material specifically comprises: providing a graphene oxide dispersion, and mixing the graphene oxide dispersion with cement, so that the graphene oxide in the graphene oxide dispersion modifies the cement;
[0010] More specifically, cement and graphene oxide are stirred at a speed of 57-67 r / min for 2-3 min, and then stirred at a speed of 115-135 r / min for 2-3 min to obtain graphene oxide modified cement;
[0011] Then, the emulsified asphalt, the defoamer and the graphene oxide modified cement are stirred at a speed of 11900-12500 r / min for 34-36 s to obtain an asphalt modified cement-based composite material.
[0012] The invention also provides an asphalt-modified cement-based composite material prepared by the preparation method.
[0013] The invention also provides application of the asphalt-modified cement-based composite material in oil and gas wells.
[0014] Compared with the prior art, the beneficial effects of the present invention are at least:
[0015] The preparation method of the asphalt-modified cement-based composite material provided by the present invention fully utilizes the advantages of the organic-inorganic system of oil well cement and emulsified asphalt, and the introduced graphene oxide further accelerates the hydration of cement and promotes the demulsification of emulsified asphalt, forming a more complete "spatial network structure" microstructure within the system, thereby greatly improving the strength, toughness and durability of the system. DETAILED DESCRIPTION
[0016] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be clearly and completely described below. It is mainly a method for preparing an asphalt-modified cement-based composite material. In addition, the asphalt-modified cement-based composite material prepared by the preparation method and the application of the asphalt-modified cement-based composite material in oil and gas wells are also provided.
[0017] As one aspect of the technical solution of the present invention, a method for preparing an asphalt-modified cement-based composite material includes:
[0018] Modifying cement with graphene oxide to obtain graphene oxide modified cement;
[0019] The emulsified asphalt, the defoamer and the graphene oxide modified cement are evenly mixed to prepare an asphalt modified cement-based composite material.
[0020] In some specific embodiments, a graphene oxide dispersion is provided, and the graphene oxide dispersion is mixed with cement, so that the graphene oxide in the graphene oxide dispersion modifies the cement.
[0021] The graphene oxide dispersion is prepared by ultrasonically dispersing graphene oxide prepared by an improved Hummer method, water and a surfactant.
[0022] Furthermore, the surfactant includes any one of β-naphthalenesulfonic acid formaldehyde and polycarboxylic acid-based high-performance water reducer or a combination of two thereof.
[0023] Furthermore, the mass ratio of the surfactant to cement is 0.15-0.60:100.
[0024] Furthermore, the ultrasonic dispersion time is 30-40 min.
[0025] More specifically, cement and graphene oxide are stirred at a speed of 57-67 r / min for 2-3 min, and then stirred at a speed of 115-135 r / min for 2-3 min to obtain graphene oxide modified cement.
[0026] Furthermore, the solid content of the graphene oxide is 2.7-3.0%, and the specific surface area is 2300-2500m 2 / g, the zeta potential is -(29-30)mV, and the main elements of graphene oxide are carbon (66.1at%) and oxygen (33.5at%).
[0027] Graphene oxide, as a typical two-dimensional flaky carbon nanomaterial, has good mechanical properties. Its Young's modulus and tensile strength are approximately 0.3TPa and 112GPa, respectively. Its aspect ratio is as high as over 30,000. Its surface is rich in oxygen-containing functional groups, making it an ideal high-strength fiber toughening material.
[0028] Furthermore, the mass ratio of the graphene oxide to cement is 0.01-0.05:100.
[0029] The cement includes high sulfate resistance oil well cement. Specifically, the cement is G-grade high sulfate resistance oil well cement required by "Test Methods for Oil Well Cement" GB / T19139-2013, and its setting time is 95 minutes, and its 8h compressive and flexural strengths are 16.7 MPa and 6.8 MPa respectively.
[0030] In some specific embodiments, the emulsified asphalt, the defoaming agent and the graphene oxide modified cement are stirred at a speed of 11900-12500 r / min for 34-36 s to obtain an asphalt modified cement-based composite material.
[0031] Furthermore, the mass ratio of the emulsified asphalt to the graphene oxide modified cement is 0.2-0.3:1, the needle penetration of the emulsified asphalt is 86, the elongation is 50, and the softening point is 56°C.
[0032] Furthermore, the needle penetration (25°C, 100g, 5s) (0.1mm) of the emulsified asphalt is 86, the elongation (5°C, 5cm / min) (cm) is 50, and the softening point is 56°C.
[0033] Furthermore, the mass ratio of the defoaming agent to the graphene oxide modified cement is 1.0-1.5:100, and the pH value of the defoaming agent is 7.0-7.5.
[0034] Furthermore, the temperature of the graphene oxide modified cement, water and emulsified asphalt is 22-24°C.
[0035] In some more specific embodiments, the method for preparing the asphalt-modified cement-based composite material comprises:
[0036] Step 1: Preparation of graphene dispersion
[0037] A high concentration of graphene oxide is prepared by an improved Hummer method; the high concentration of graphene oxide is then diluted with deionized water, stirred at a constant speed for 1 minute with a glass rod during the dilution process, and then treated with a surfactant combined with ultrasonic dispersion for 30 minutes to obtain a highly dispersed and stable graphene dispersion.
[0038] Step 2: Preparation of graphene oxide modified cement
[0039] The cement and the diluted graphene oxide suspension were mechanically stirred with a cement slurry mixer at an orbital speed of 57-67 r / min for 2 min, and then at an orbital speed of 115-135 r / min for 2 min to obtain a uniform mixture.
[0040] Step 3: Preparation of asphalt-modified cement-based composites
[0041] The prepared emulsified asphalt and defoamer solution are added to the uniform mixture, and then mechanically stirred at an orbital speed of 11900-12500 r / min for 34-36 seconds to obtain an asphalt-modified cement-based composite material for oil and gas wells.
[0042] The technical principle of the present invention is that graphene oxide is a carbon-based nanomaterial with a large specific surface area, and its surface is rich in oxygen functional groups. It is an ideal cement-based reinforcement and toughening material, and the key to the enhancement effect of graphene oxide is to fully disperse it in the cement matrix. This technical solution adopts the self-designed "physics + chemistry, that is, ultrasound + surfactant treatment" combined with a dispersion process to prepare a highly dispersed graphene oxide suspension; two-dimensional flake graphene oxide can significantly enhance the strength of oil well cement; on this basis, organic emulsified asphalt is introduced, and the hydration of cement consumes the water of emulsified asphalt. At the same time, it can accelerate the demulsification of emulsified asphalt, and finally form a "spatial network structure" in which the asphalt film and cement hydration products are interspersed. In addition, due to the presence of flake two-dimensional graphene oxide in the cement matrix, the system's crack initiation and expansion inhibition effect is further increased, and the deformation capacity of the system is synergistically increased, thereby greatly improving the toughness of the system and greatly improving the early strength of the system. In addition, nano-scale graphene oxide can also accelerate cement hydration and fill the "vacancies" left over from emulsified asphalt demulsification and water evaporation, thereby compacting the microstructure, which is the key to improving the strength and durability of the system.
[0043] Another aspect of the technical solution of the present invention provides an asphalt-modified cement-based composite material prepared by the preparation method, wherein the water-cement ratio of the asphalt-modified cement-based composite material is 0.45.
[0044] In addition, another aspect of the embodiments of the present invention further provides the use of the asphalt-modified cement-based composite material in oil and gas wells.
[0045] In summary, the preparation method of the asphalt-modified cement-based composite material of the present invention can achieve a significant improvement in the toughness of the cement ring. With graphene oxide, oil well cement and emulsified asphalt as main raw materials, through composite modification treatment, while giving full play to the advantages of the organic-inorganic system of oil well cement and emulsified asphalt, the introduced graphene oxide further accelerates the hydration of cement and promotes the demulsification of emulsified asphalt, forming a more complete "spatial network structure" microstructure inside the system, and the prepared asphalt-modified cement-based composite material has excellent toughness and deformation ability.
[0046] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on them. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.
[0047] Example 1
[0048] This embodiment provides a method for preparing an asphalt-modified cement-based composite material, comprising the following steps:
[0049] Step 1: Preparation of graphene dispersion
[0050] A high concentration of graphene oxide is prepared by an improved Hummer method; the high concentration of graphene oxide is then diluted with deionized water, stirred at a constant speed for 1 minute with a glass rod during the dilution process, and then ultrasonic dispersion is used for 30 minutes combined with surfactant treatment to obtain a highly dispersed and stable graphene dispersion.
[0051] Step 2: Preparation of graphene oxide modified cement
[0052] The cement and the diluted graphene oxide suspension were mechanically stirred with a cement slurry mixer at an orbital speed of 57 r / min for 2 min, and then at an orbital speed of 115 r / min for 2 min to obtain a uniform mixture.
[0053] Step 3: Preparation of asphalt-modified cement-based composites
[0054] The prepared emulsified asphalt and defoamer solution are added to the uniform mixture, and then mechanically stirred at an orbital speed of 11900 r / min for 34-36 seconds to obtain an asphalt-modified cement-based composite material for oil and gas wells.
[0055] The surfactant is β-naphthalenesulfonic acid formaldehyde, with a solid content of 95% and an amount of 0.15% (based on the mass ratio of cement). The concentration of the diluted graphene dispersion is 1 mg / mL.
[0056] The cement is the G-grade high sulfate-resistant oil well cement required by the "Test Methods for Oil Well Cement" GB / T19139-2013, with a setting time of 95 minutes, and 8-hour compressive and flexural strengths of 16.7 MPa and 6.8 MPa, respectively.
[0057] The needle penetration (25°C, 100g, 5s) (0.1mm) of the emulsified asphalt is 86, the ductility (5°C, 5cm / min) (cm) is 50, and the softening point is 56°C. The concentration of the defoamer solution is 1.5% (based on the mass ratio of cement), the solid content is 60%, and the pH is 7.2.
[0058] The water-cement ratio of the mixture is 0.45, the amount of graphene oxide used is 0.03% of the mass of cement, and the mass ratio of emulsified asphalt to cement (solid content) is 0.25. The raw material temperatures of cement, water and emulsified asphalt are all 22°C, and deionized water is used.
[0059] Example 2
[0060] This embodiment provides a method for preparing an asphalt-modified cement-based composite material for oil and gas wells, and the steps are basically the same as those in Example 1, except that the amount of graphene oxide used is 0.01% of the mass of cement.
[0061] Example 3
[0062] This embodiment provides a method for preparing an asphalt-modified cement-based composite material for oil and gas wells, and the steps are basically the same as those in Example 1, except that the amount of graphene oxide used is 0.05% of the mass of cement.
[0063] Example 4
[0064] This embodiment provides a method for preparing an asphalt-modified cement-based composite material for oil and gas wells. The steps are basically the same as those in Example 1, except that the mass ratio (solid content) of emulsified asphalt to cement is 0.2:1.
[0065] Example 5
[0066] This embodiment provides a method for preparing an asphalt-modified cement-based composite material for oil and gas wells. The steps are basically the same as those in Example 1, except that the mass ratio (solid content) of emulsified asphalt to cement is 0.3:1.
[0067] Example 6
[0068] This embodiment provides a method for preparing an asphalt-modified cement-based composite material, comprising the following steps:
[0069] Step 1: Preparation of graphene dispersion
[0070] A high concentration of graphene oxide was prepared by an improved Hummer method; the high concentration of graphene oxide was then diluted with deionized water, stirred at a constant speed for 1 minute with a glass rod during the dilution process, and then ultrasonic dispersion was used for 40 minutes combined with surfactant treatment to obtain a highly dispersed and stable graphene dispersion.
[0071] Step 2: Preparation of graphene oxide modified cement
[0072] The cement and the diluted graphene oxide suspension were mechanically stirred with a cement slurry mixer at an orbital speed of 67 r / min for 3 min, and then at an orbital speed of 135 r / min for 3 min to obtain a uniform mixture.
[0073] Step 3: Preparation of asphalt-modified cement-based composites
[0074] The prepared emulsified asphalt and defoamer solution are added to the uniform mixture, and then mechanically stirred at a revolution speed of 12500 r / min for 34-36 seconds to obtain an asphalt-modified cement-based composite material for oil and gas wells.
[0075] The surfactant is a polycarboxylic acid-based high-performance water-reducing agent, with a solid content of 95% and a dosage of 0.10% (based on the mass ratio of cement). The concentration of the diluted graphene dispersion is 1 mg / mL.
[0076] The cement is the G-grade high sulfate-resistant oil well cement required by the "Test Methods for Oil Well Cement" GB / T19139-2013, with a setting time of 95 minutes, and 8-hour compressive and flexural strengths of 16.7 MPa and 6.8 MPa, respectively.
[0077] The needle penetration (25°C, 100g, 5s) (0.1mm) of the emulsified asphalt is 86, the ductility (5°C, 5cm / min) (cm) is 50, and the softening point is 56°C. The concentration of the defoamer solution is 1.5% (based on the mass ratio of cement), the solid content is 60%, and the pH is 7.5.
[0078] The water-cement ratio of the mixture is 0.45, the amount of graphene oxide used is 0.03% of the mass of cement, and the mass ratio of emulsified asphalt to cement (solid content) is 0.25. The raw material temperatures of cement, water and emulsified asphalt are all 24°C, and deionized water is used.
[0079] Comparative Example 1
[0080] In this comparative example, a pure oil well cement slurry is provided.
[0081] Pure oil well cement slurry can be obtained by mechanically stirring oil well cement and water at an orbital speed of 11900r / min for 34s.
[0082] Comparative Example 2
[0083] This comparative example provides an emulsified asphalt modified oil well cement slurry.
[0084] The oil well cement, water and emulsified asphalt are mechanically stirred at a revolution speed of 11900 r / min for 34 seconds to obtain an emulsified asphalt modified oil well cement slurry. The mass ratio (solid content) of emulsified asphalt to cement is 0.25.
[0085] Comparative Example 3
[0086] This comparative example provides a graphene oxide modified cement slurry.
[0087] The cement and graphene oxide suspension were mechanically stirred with a cement slurry mixer at an orbital speed of 57 r / min for 2 min, and then at an orbital speed of 115 r / min for 2 min to obtain a uniform mixture.
[0088] Comparative Example 4
[0089] This comparative example provides a graphene oxide modified cement slurry.
[0090] The cement and graphene suspension were mechanically stirred with a cement slurry mixer at an orbital speed of 57 r / min for 2 min, and then at an orbital speed of 115 r / min for 2 min to obtain a uniform mixture.
[0091] Comparative Example 5
[0092] This comparative example provides a graphene oxide modified cement slurry.
[0093] The cement and the graphene oxide aqueous solution (without surfactant) were mechanically stirred with a cement slurry mixer at an orbital speed of 57 r / min for 2 min, and then at an orbital speed of 115 r / min for 2 min to obtain a uniform mixture.
[0094] The performance test of the asphalt-modified cement-based composite material for oil and gas wells provided in the above embodiment is shown in the following table:
[0095]
[0096] Refer to GB / T19139-2013 "Oil Well Cement Materials and Test Specifications" to prepare and maintain oil well cement slurry. Then pour the prepared cement slurry into the cylindrical steel mold. The compressive strength was measured after 1 and 28 days of curing, and the final compressive strength value was the average of 5 specimens. According to the Brazilian splitting tensile strength method, the cement paste was injected into the cylindrical mold. After reaching the preset curing age, the splitting tensile strength of cement paste is tested (average value of 5 specimens). The flexural strength of the samples was tested using a rock mechanics testing system with a loading rate of 2 kN / min. The final flexural strength was the average value of 5 samples.
[0097] Results Analysis
[0098] Based on the above embodiments and test results, it can be clearly seen that the asphalt-modified cement-based composite material for oil and gas wells provided by the present invention makes full use of the respective characteristics of organic (emulsified asphalt) and inorganic (oil well cement), and combines the use of graphene oxide to greatly increase the early strength and toughness (tensile and flexural strength) of the system.
[0099] It can be seen from Comparative Example 1, Example 2 and Example 3 that there is an optimal amount of graphene oxide for the improvement of cement strength, which is about 0.03% of the mass of cement; similarly, from Comparative Example 1, Example 4 and Example 5, it can be seen that the optimal ratio of emulsified asphalt to cement mass ratio (solid content) is 0.25. It can be seen from Comparative Example 1 and Comparative Example 2 that the introduction of emulsified asphalt can increase the 1d and 28d tensile strengths of the system by about 20% and 12.5%, respectively, while reducing its 1d and 28d compressive strengths by 8.9% and 8.3%, respectively. It can be seen from Comparative Example 1 and Comparative Example 2 that the introduction of graphene oxide can greatly improve the mechanical properties of the system, specifically, its 1d compressive strength, 1d tensile strength and 1d flexural strength are increased by about 45%, 30% and 35%, respectively. And the 28d strength is greatly improved. It can be seen from Comparative 1-Comparative 5 that the graphene oxide dispersion pretreated with a surfactant has a significant positive effect on improving the strength of cement-based composite materials.
[0100] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0101] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing an asphalt-modified cement-based composite material, characterized in that include: Provided is a graphene oxide dispersion, wherein the graphene oxide dispersion is prepared by ultrasonically dispersing graphene oxide, water and a surfactant, wherein the solid content of the graphene oxide is 2.7-3.0%, and the specific surface area is 2300-2500m 2 / g, zeta potential is -(29-30)mV, main elements of graphene oxide are 66.1at% carbon and 33.5at% oxygen, the surfactant is selected from any one or a combination of two of β-naphthalenesulfonic acid formaldehyde and polycarboxylic acid-based high-performance water reducer, and the mass ratio of the surfactant to cement is 0.15-0.60:100; The graphene oxide dispersion is mixed with cement, and the cement and graphene oxide are stirred at a speed of 57-67 r / min for 2-3 min, and then stirred at a speed of 115-135 r / min for 2-3 min, so that the graphene oxide in the graphene oxide dispersion modifies the cement to obtain graphene oxide modified cement; the mass ratio of graphene oxide to cement in the graphene oxide dispersion is 0.01-0.05:100; The emulsified asphalt, the defoamer and the graphene oxide modified cement are uniformly mixed to obtain an asphalt modified cement-based composite material; the mass ratio of the emulsified asphalt to the graphene oxide modified cement is 0.2-0.3:1, the mass ratio of the defoamer to the graphene oxide modified cement is 1.0-1.5:100, and the pH value of the defoamer is 7.0-7.5; the temperature of the graphene oxide modified cement and the emulsified asphalt is 22-24°C.
2. The preparation method according to claim 1, characterized in that: The ultrasonic dispersion time is 30-40 min.
3. The preparation method according to claim 1, characterized in that: The cement is selected from high sulfate-resistant oil well cement.
4. The preparation method according to claim 1, characterized in that Specifically include: The emulsified asphalt, defoamer and graphene oxide modified cement were stirred at a speed of 11900-12500 r / min for 34-36 s to obtain an asphalt modified cement-based composite material.
5. An asphalt-modified cement-based composite material prepared by the preparation method according to any one of claims 1 to 4.
6. The asphalt-modified cement-based composite material according to claim 5, characterized in that: The water-cement ratio of the asphalt-modified cement-based composite material is 0.
45.