Well cementation cement slurry system capable of resisting ultrahigh temperature of 240 DEG C
By adding specific additives to the cement slurry to adjust the structure of the hydrated product, the problem of strength decay of high-temperature cement cement at an environment above 240°C is solved, and the high strength and toughness of cement stone is achieved to ensure the integrity and stability of the wellbore.
Patent Information
- Application Number
- CN202411042266.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high-temperature cement strength decay problem in ultra-high temperature environments has not been effectively solved, resulting in the damage to the integrity of the wellbore, and it is difficult for the existing technology to maintain stable compressive strength and toughness in an environment above 240°C.
By adding strength stabilizers, anti-strength decayers, lattice growth inhibitors and structural stabilizers to the cement slurry, the morphology and structure of the hydration products are adjusted, combined with retarders, dehydration agents, suspension stabilizers and digestion Foaming agent forms a high-strength and high-strength cement slurry system to ensure the compactness and mechanical properties of cement stone.
The compressive strength and elastic modulus of cement stone were significantly improved. The compressive strength exceeded 56.3MPa after 7 days of maintenance under 240℃, and exceeded 61MPa after 14 days, and there was no significant decline in 28d and 40d, achieving the high strength and high toughness of cement stone. And ensure the integrity of the wellbore.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of deep oil and gas drilling and completion, and in particular to a 240°C ultra-high temperature resistant cementing slurry system. Background Art
[0002] At present, 57.48% of the world's energy supply comes from oil and natural gas. In order to increase and stabilize production, major domestic oil fields are exploring and developing deeper strata in old blocks. According to statistics, my country's deep oil and gas resources amount to 671×10 8 t, accounting for more than 34% of the total oil and gas resources. Deep oil and gas resources have become a major replacement energy source for oil and gas in my country. The exploitation of these deep and ultra-deep wells still faces a series of challenges, especially the poor mechanical properties of cement stone under high and ultra-high temperature environments.
[0003] The high temperature and high pressure downhole environment will cause the phase change of cement hydration products, which may cause serious deterioration of material strength. Under the combined effect of high temperature and high pressure, the compressive strength of cement paste will decline to varying degrees, thus destroying the integrity of the wellbore. At present, the main way to solve the decline in the compressive strength of high temperature cement paste is to add 30% to 50% silica sand to oil well cement, and to enhance the strength stability of cement paste at high temperature and improve the mechanical properties of cement paste by adjusting the calcium-silicon ratio of the cement slurry system and improving the types and crystal structures of hydration products. However, indoor studies have shown that the compressive strength of commonly used silica sand cement paste reaches 52MPa after curing at 180℃ and 20MPa for 14 days, while the compressive strength of the same formula after curing at 210℃ and 20MPa for 14 days is only 6.65MPa, and the permeability increases sharply, and the long-term sealing performance of the cement ring cannot be guaranteed. With the continuous advancement of my country's oil and gas exploration and development to increase reserves and production, higher requirements are put forward for the mechanical properties of cement rings in complex wellbore environments, and high temperature resistant cement slurry systems have become a research hotspot.
[0004] Chinese patent CN109761547A discloses a cement slurry system suitable for large-scale staged fracturing of shale gas horizontal wells. The technology modifies the surface of rubber particles to enhance hydrophilicity, and the elastic modulus of cement stone is less than 6GPa. However, the temperature resistance of rubber particles is poor, and it is difficult to apply them to high-temperature deep well cementing at 240°C.
[0005] Chinese invention patent CN108675752A discloses a high-strength, high-temperature, and erosion-resistant cement and a preparation method thereof. The main components of the oil well cement are G-grade high-resistance oil well clinker, phosphate aluminate cement clinker, silica sand, phosphogypsum, silica powder, fluid loss reducer, and retarder. The oil well cement can be used at a temperature of up to 300°C, but has a short thickening time and is unstable when a special retarder is added, making it impractical.
[0006] The prior art Chinese invention patent CN109679600A discloses a nanomaterial mixed modified ultra-high temperature high performance cementing slurry system and its preparation method. The combination of coarse and fine silica sand, nano silicon dioxide and nano calcium carbonate can improve the mechanical properties of high temperature cement paste, with a 5-day strength of 60MPa and an elastic modulus of about 8.5, but long-term strength decay (more than 28 days) will occur at high temperatures above 240°C.
[0007] The prior art Chinese invention patent CN107902933A discloses an oil well cement anti-high temperature decay admixture and its preparation method. The main components of the cement slurry system include photovoltaic silicon, fumed silica, dead-burned magnesium oxide and mineral fiber materials, which effectively ensure the compressive strength above 200°C and achieve the effect of reducing the decay of compressive strength. However, its 28d strength is only 37.8MPa, and the high temperature resistance and compressive strength performance needs to be further improved.
[0008] In summary, the existing high-temperature cementing cement strength decay suppression technology still has shortcomings, mainly because the complex hydration process and microstructure of the silicate cement system are difficult to control, resulting in a decrease in the macroscopic strength of the cement paste. Simply controlling the silicon-calcium ratio, particle grading, or improving the density of the cement paste cannot fundamentally solve the problem of strength decay of oil well cement in ultra-high temperature environments. Therefore, finding and improving methods to prevent the strength decay of cement for well cementing is still a major key problem in oil and gas exploration and development projects. Summary of the invention
[0009] The present invention aims at the problem that cementing cement has low strength, poor toughness and the integrity of the wellbore is seriously damaged in the later operation. Based on the existing research on the control of cementing cement hydration process, the regulation of multi-level microstructure of hydration products and the improvement of mechanical properties, the present invention adds four key additives, namely strength stabilizer, strength decay resistance agent, lattice growth inhibitor and structure stabilizer, to cement slurry, which can effectively regulate the morphology, type and accumulation state of hydration products at different scales and different hydration stages, thereby effectively regulating the microstructure and hydration products of cement stone, and finally significantly improving the mechanical properties of cement stone. The cement slurry system that can meet the ultra-high temperature cementing operation is formed by cooperating with the retarder, fluid loss reducer, suspension stabilizer, drag reducer and defoamer.
[0010] In order to form a high-strength and high-toughness structure of cement stone, this patent adds structural stabilizers and lattice growth inhibitors to cementing cement slurry. The former forms a mesh structure in the cement slurry matrix at the early stage of cement hydration at the micrometer scale, exerting a bridging and pull-out effect. The latter fills the microscopic pores of cement stone at the nanometer scale on the one hand, exerting a physical filling effect, and on the other hand forms a spatial resistance to prevent the transformation of the hydration product from a columnar structure to a parallel needle-rod structure. The synergistic effect of the two ensures the density of the microstructure of cement stone and the hydration product at different scales.
[0011] In order to improve the formation of hydration products, this patent adds strength stabilizers and anti-strength decay agents to the cementing cement slurry. Compared with conventional quartz sand, the quartz sand in the strength stabilizer is prepared from high-purity vein quartz and is acid-washed, which further increases the content of hydrated calcium silicate in the early stage of hydration. The anti-strength decay agent undergoes secondary hydration reaction with cement in the middle and late stages of hydration to generate a high-temperature stable product, alumina-silicate, which inhibits the formation of parallel needle-shaped xonotlite. The synergistic effect of the two promotes the formation of high-temperature stable hydration products at different hydration stages and inhibits the formation of fragile hydration deposition products.
[0012] In order to achieve the object of the present invention, the technical solution of the present invention is as follows:
[0013] The invention provides a 240°C ultra-high temperature resistant cementing slurry system, comprising the following components in parts by mass: 100 parts of oil well G-grade cement, 30-50 parts of strength stabilizer, 5-15 parts of anti-strength decay agent, 0.3-1 parts of lattice growth inhibitor, 1-3 parts of structure stabilizer, 0.5-5 parts of suspension stabilizer, 0.5-5 parts of retarder, 4-10 parts of fluid loss reducer, 1-3 parts of drag reducer, 0.2-1 parts of defoamer and 38-60 parts of water.
[0014] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the quartz sand in the strength stabilizer is produced from vein quartz, the vein quartz is crystalline, and the mass fraction of silicon dioxide is above 99.5%. The specific preparation process is as follows: the vein quartz is initially crushed into quartz particles of 50 to 80 meshes; concentrated hydrochloric acid with a mass fraction of 25 to 37% and hydrofluoric acid with a mass fraction of 5 to 20% and water with a volume ratio of 10 to 15:1 to 2:10 to 17 are mixed to prepare an acid solution, acid leaching is performed at room temperature for 10 to 12 hours, and stirring is performed at a speed of 100 to 150 r / min; impurities in coarse ore particles are removed by water washing; a ball mill is used to grind with a material-ball ratio of 1:2, a water addition ratio of 40 to 50%, and a ball milling time of 30 to 50 minutes, and then quartz sand with a particle size of 100 to 200 meshes is screened out as coarse quartz sand, and quartz sand with a particle size of 400 to 500 meshes is screened out as fine quartz sand, and the two quartz sands are evenly mixed at a mass fraction of 23 to 30:35 to 47 to obtain a strength stabilizer. Preferably, the coarse quartz sand and fine quartz sand are white solid powders with a density between 2.65 and 2.70 g / cm 3 , the purity is above 99.5%.
[0015] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the lattice growth inhibitor is mainly a nano-scale one-dimensional chemically inert material, which plays a physical filling role in filling microscopic pores to increase the density of cement stone, and plays a crystal nucleus role of the nano material on the other hand, optimizes the nucleation site of the hydration product at low temperature, promotes the hydration reaction, and forms a spatial resistance at high temperature to prevent the hydration product from transforming from a columnar structure to a parallel needle-rod structure; the lattice growth inhibitor is obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide in a mass fraction of 20-43:15-37:25-55, wherein the particle size of the nano calcium carbonate is between 60-80 nm, the particle size of the nano titanium dioxide is between 40-80 nm, and the particle size of the nano zirconium dioxide is between 30-70 nm.
[0016] The described 240°C ultra-high temperature resistant cementing slurry system, wherein the described strength decay resistance agent is mainly a silicoalumina material, which can generate a high-temperature stable hydration product alumina calcium silicate with cement under high-temperature hydrothermal conditions; characterized in that the described strength decay resistance agent is obtained by uniformly mixing metakaolin, zeolite, bauxite and mullite in a mass fraction of 5-10:12-27:17-32:28-37, wherein the metakaolin particle size is between 40 and 50 μm, the zeolite particle size is between 75 and 106 μm, the bauxite particle size is between 58 and 75 μm, and the mullite particle size is between 48 and 75 μm.
[0017] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the structural stabilizer has the characteristics of large aspect ratio, high mechanical strength and high temperature resistance, can be bridged between the cement hydration products of the oil well to build a three-dimensional staggered layered structure, and play the role of "pulling out" and "crack deflection". The specific preparation process of the crystal enhancer is to add 20 to 35 parts of inorganic single crystal materials and 5 to 12 parts of fiber materials in 100 parts of deionized water under stirring conditions of 200 to 300 rpm, and then add 8 to 15 parts of tetraethyl orthosilicate, adjust the pH to 5.0 to 6.0 with dilute hydrochloric acid, then heat to 60 to 65°C, continue to react for 50 to 80 minutes under stirring, cool to room temperature, filter, and put into a 100 to 105°C oven for drying for 18 to 24 hours to obtain the crystal enhancer. Preferably, the inorganic single crystal material is one or a combination of calcium carbonate, aluminum borate and magnesium silicate inorganic single crystal materials, and the fiber material is one or a combination of carbon fiber and basalt fiber.
[0018] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the fluid loss reducer is obtained by free radical copolymerization of N,N-dimethylacrylamide (NNDMA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS), sodium styrene sulfonate (SSS) and itaconic acid (IA) in a mass fraction of 27-40:24-38:10-16:18-27 in pure water at 50-55°C through a sodium bisulfite-ammonium persulfate initiator system, wherein the reaction pH is 5.5-6.5 and the reaction time is 240-300 minutes.
[0019] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the retarder is obtained by free radical copolymerization of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N,N-dimethylacrylamide (DMAA), acrylic acid (AA), and vinylphosphonic acid (VPA) in a mass fraction of 17-30:12-28:25-46:28-57 in pure water at 40-45°C with a hydrogen peroxide initiator, wherein the reaction pH is 3.0-3.5 and the reaction time is 360-480 minutes.
[0020] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the suspension stabilizer is obtained by uniformly mixing solid powder of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N,N-dimethylacrylamide (DMAA), and sodium styrene sulfonate (SSS) copolymer with nano-attapulgite and magnesium aluminum silicate in a mass fraction of 37-60:9-21:12-28.
[0021] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the drag reducer is one of a sulfonated aldehyde ketone polycondensate drag reducer, a naphthalene sulfonate drag reducer, and a polycarboxylic acid drag reducer, or a mixture thereof.
[0022] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the defoamer is one of a phosphate defoamer, an organosiloxane defoamer, an organic polyether defoamer, and an organosilicon ether defoamer, or a mixture thereof.
[0023] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the oil well cement is G-grade oil well cement or H-grade oil well cement.
[0024] The 240°C ultra-high temperature resistant cementing slurry system is characterized in that the water is fresh water or low-mineralization water.
[0025] According to the present invention, the 240°C ultra-high temperature resistant cementing slurry system is determined according to relevant industry standards, and the types and amounts of four key additives can be optimized according to the on-site use environment and requirements, and the amounts of materials such as fluid loss reducer, drag reducer, retarder, defoamer, etc. can be optimized, and the engineering properties such as water loss, rheological parameters, and thickening time of the cement slurry system can be optimized and adjusted to meet the on-site construction requirements of cementing.
[0026] According to the present invention, the above-mentioned 240°C ultra-high temperature resistant cementing slurry system comprises the following steps:
[0027] The oil well cement, strength stabilizer, structural stabilizer, anti-strength decay inhibitor, lattice growth inhibitor, suspension stabilizer and drag reducer are mixed evenly, and the retarder, fluid loss reducer, water and defoamer are poured into the stirring slurry cup of the constant speed stirrer. Within 15 seconds, the solid phase material is continuously and evenly poured into the stirring slurry cup at a speed of 4000 rpm to mix with the liquid phase material, and then the speed is adjusted to 12000 rpm. After stirring for 35 seconds, a 240°C ultra-high temperature resistant cementing slurry system can be obtained.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The strength stabilizers used in the 240°C ultra-high temperature resistant cementing slurry system of the present invention are all homemade in the laboratory. The raw materials are vein quartz with a high silica content, which is obtained through acid washing and other treatments. Compared with traditional quartz sand, it has fewer impurities, higher silica content, more obvious micro-aggregate effect, and more uniform hydration products. In addition, the quartz sand, cement strength decay resistance agent and other solid materials are closely packed together to increase the solid content per unit volume of the ultra-high temperature resistant cementing slurry.
[0030] 2. The 240°C ultra-high temperature cementing slurry system of the present invention has the characteristics of high strength and high toughness. After curing at 240°C, the compressive strength of the cement paste is greater than 56.3MPa after 7 days, and the compressive strength of the cement paste is greater than 61MPa after 14 days. There is no obvious decline in the compressive strength of the cement paste at 28 days and 40 days, and the elastic modulus at 14 days is 4.0GPa, achieving the goal of high strength and high toughness of the cement paste.
[0031] 3. The 240°C ultra-high temperature resistant cementing slurry system of the present invention has good rheology, stable slurry, low filtration loss, and the four key additives required are widely available and inexpensive, and can play the designed role within a relatively wide range of addition, which is convenient for construction operations;
[0032] 4. The 240°C ultra-high temperature resistant cementing slurry system of the present invention can be applied to deep wells / ultra-deep wells and a wider range of high-temperature formation cementing scenarios, can ensure the integrity of the cement ring, effectively isolate the formation, and has a very broad application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 These are scanning electron microscope images of cement slurries of Comparative Example 1 and Example 1 cured at 240°C for 7 days. The cement paste formed by adding strength stabilizer, structural stabilizer, strength decay inhibitor and lattice growth inhibitor has a denser microstructure, and the hydration products are arranged more orderly, presenting a tighter structure (Scanning electron microscope images of cement paste cured at 240°C for 7 days, the left is Comparative Example 1, and the right is Example 1).
[0034] Figure 2 The hydration heat release rate curve of cement slurry hydration process of comparative example 1 and example 1. The addition of strength stabilizer, structure stabilizer, anti-strength decay inhibitor and lattice growth inhibitor leads to a significant increase in heat release rate and peak value of each peak (Scanning electron microscope image of cement stone cured at 240°C for 7 days, the left is comparative example 1, and the right is example 1).
[0035] Figure 3 The cumulative heat release curve of hydration heat of comparative example 1 and example 1. Example 1 releases more heat during the hydration process than comparative example 1, indicating that more hydration products are formed (the cumulative heat release curve of hydration heat, the solid line is comparative example 1, and the dotted line is example 1). DETAILED DESCRIPTION
[0036] The present invention is further described below by means of specific examples and comparative examples, but is not limited thereto.
[0037] Experimental method: A cement slurry system resistant to ultra-high temperature of 240°C was prepared according to the standard GB / T 19139-2012 "Test methods for oil well cement", and the performance of a cement slurry system resistant to ultra-high temperature of 240°C was tested according to the standard SY / T 6544-2017 "Performance requirements for oil well cement slurries".
[0038] The sources and properties of the raw materials used in the following examples and comparative examples are as follows:
[0039] Oil well cement: Use Grade G oil well cement from Weifang Shengwei Special Cement Co., Ltd.
[0040] Vein quartz: purchased from Kasong Quartz Sand Factory in Jianping County, Liaoning Province, it is formed by the hot water solution secreted from underground magma filling and precipitating in the cracks of the rock. The quartz is crystalline, with a silicon dioxide content of more than 99.5% and a density of 2.65-2.70g / cm 3 between.
[0041] Nano calcium carbonate: purchased from Yuxin Nanotechnology Co., Ltd., with a calcium carbonate mass fraction greater than 93%, a particle size between 60 and 80 nm, and a specific surface area of 21 to 25 m 2 / g, activation degree is greater than 99.9%.
[0042] Nano titanium dioxide: purchased from Hangzhou Hengna New Materials Co., Ltd., white loose powder, rutile crystal form, rutile content greater than 99.9%, particle size between 40 and 80 nm.
[0043] Nano zirconium dioxide: purchased from Hangzhou Hengna New Materials Co., Ltd., white powder, tetragonal crystal phase, particle size between 30 and 70 nm.
[0044] Metakaolin: purchased from Shandong Qiyi Chemical Technology Co., Ltd., with a particle size between 40 and 50 μm.
[0045] Zeolite: purchased from Shenyang Loncin Mineral Products Co., Ltd., with a particle size between 75 and 106 μm.
[0046] Bauxite: purchased from Gongyi Songfeng Mining Industry Co., Ltd., with a particle size between 58 and 75 μm and an alumina content between 70 and 86%.
[0047] Mullite: purchased from Shandong Jinda Technology New Materials Co., Ltd., with a particle size between 48 and 75 μm and an alumina content between 42 and 46%.
[0048] Ethyl orthosilicate: purchased from Shandong Sike New Materials Co., Ltd., a colorless transparent liquid, melting point: -82.49°C, boiling point: 168°C, relative density: 0.934 g / cm 3 , flash point: 45℃, auto-ignition temperature: 222℃.
[0049] Carbon fiber: purchased from Jilin Chemical Fiber Group Co., Ltd., with an elastic modulus greater than 235 GPa and a carbon content greater than 93%.
[0050] Basalt fiber: purchased from Changzhou Yibao New Material Technology Co., Ltd., with a fiber density of 2.6-2.8 g / cm 3 , the fiber length is 5 to 15 mm, and the breaking strength is greater than 1500 MPa.
[0051] Drag reducer: HX-21L drag reducer for oil well cement produced by Chengdu OMEC Petroleum Technology Co., Ltd.
[0052] Defoaming agent: Chengdu OMEC Petroleum Technology Co., Ltd., defoaming agent DF-A for oil well cement is used.
[0053] Example 1
[0054] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 30 parts of strength stabilizer, 5 parts of anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite at a mass fraction of 10:12:17:28), 0.3 parts of lattice growth inhibitor (obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide at a mass fraction of 20:37:55), 1 part of structural stabilizer (obtained by calcium carbonate whiskers and carbon fiber), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 1 part of drag reducer, 1 part of defoamer and 44 parts of water.
[0055] A 240°C ultra-high temperature resistant cementing slurry system comprises the following steps:
[0056] According to the standards GB / T 19139-2012 "Test methods for oil well cement" and GB / T 33294-2016 "Test methods for deepwater oil well cement", G-grade oil well cement, strength stabilizer, anti-strength decay agent, lattice growth inhibitor, structural stabilizer, suspension stabilizer and drag reducer are mixed evenly, and retarder, fluid loss reducer, water and defoamer are poured into the mixing slurry cup of a constant speed stirrer. Within 15 seconds, the solid phase material is continuously and evenly poured into the mixing slurry cup at a speed of 4000rmp to mix with the liquid phase material, and then the speed is adjusted to 12000rmp. After stirring for 35 seconds, a cement slurry resistant to ultra-high temperature of 240°C can be obtained.
[0057] Example 2
[0058] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 40 parts of strength stabilizer, 10 parts of anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite at a mass fraction of 10:12:17:28), 0.6 parts of lattice growth inhibitor (obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide at a mass fraction of 20:37:55), 2 parts of structural stabilizer (obtained by calcium carbonate whiskers and carbon fiber), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 1.5 parts of drag reducer, 1 part of defoamer and 44 parts of water.
[0059] The preparation method is the same as that of Example 1.
[0060] Example 3
[0061] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 50 parts of strength stabilizer, 15 parts of anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite at a mass fraction of 10:12:17:28), 1 part of lattice growth inhibitor (obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide at a mass fraction of 20:37:55), 3 parts of structural stabilizer (obtained by calcium carbonate whiskers and carbon fiber), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 2 parts of drag reducer, 1 part of defoamer and 44 parts of water.
[0062] The preparation method is the same as that of Example 1.
[0063] Example 4
[0064] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 30 parts of strength stabilizer, 5 parts of anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite at a mass fraction of 5:27:32:37), 0.3 parts of lattice growth inhibitor (obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide at a mass fraction of 43:15:25), 1 part of structural stabilizer (obtained by magnesium silicate whisker and basalt fiber), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 1 part of drag reducer, 1 part of defoamer and 44 parts of water.
[0065] Example 5
[0066] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 30 parts of strength stabilizer, 5 parts of anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite in a mass fraction of 10:12:17:28), 1 part of structural stabilizer (obtained from calcium carbonate whiskers and carbon fibers), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 1 part of drag reducer, 1 part of defoamer and 44 parts of water.
[0067] Example 6
[0068] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G-grade cement, 30 parts of strength stabilizer, 0.3 parts of lattice growth inhibitor (nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide are uniformly mixed in a mass fraction of 20:37:55), 1 part of structural stabilizer (calcium carbonate whiskers and carbon fibers), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss additive, 1 part of drag reducer, 1 part of defoaming agent and 44 parts of water.
[0069] Example 7
[0070] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 30 parts of strength stabilizer, 5 parts of anti-strength decay agent (metakaolin, zeolite, bauxite and mullite are uniformly mixed at a mass fraction of 10:12:17:28), 0.3 parts of lattice growth inhibitor (nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide are uniformly mixed at a mass fraction of 20:37:55), 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss reducer, 1 part of drag reducer, 1 part of defoamer and 44 parts of water.
[0071] Example 8
[0072] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G-grade cement, 5 parts of an anti-strength decay agent (obtained by uniformly mixing kaolin, zeolite, bauxite and mullite at a mass fraction of 10:12:17:28), 0.3 parts of a lattice growth inhibitor (obtained by uniformly mixing nano-calcium carbonate, nano-titanium dioxide and nano-zirconium dioxide at a mass fraction of 20:37:55), 1 part of a structural stabilizer (obtained by calcium carbonate whiskers and carbon fibers), 4 parts of a suspension stabilizer, 3 parts of a retarder, 5 parts of a fluid loss reducer, 1 part of a drag reducer, 1 part of a defoaming agent and 44 parts of water.
[0073] Example 9
[0074] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by weight: 100 parts of oil well G-grade cement, 30 parts of strength stabilizer, 4 parts of suspension stabilizer, 3 parts of retarder, 5 parts of fluid loss additive, 1 part of drag reducer, 1 part of defoamer and 44 parts of water.
[0075] The preparation method is the same as that of Example 1.
[0076] Example 10
[0077] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G grade cement, 5 parts of an anti-strength decay agent (metakaolin, zeolite, bauxite and mullite are uniformly mixed in a mass fraction of 10:12:17:28), 4 parts of a suspension stabilizer, 3 parts of a retarder, 5 parts of a fluid loss reducer, 1 part of a drag reducer, 1 part of a defoaming agent and 44 parts of water.
[0078] The preparation method is the same as that of Example 1.
[0079] Embodiment 11
[0080] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by mass: 100 parts of oil well G-grade cement, 0.3 parts of a lattice growth inhibitor (nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide are uniformly mixed in a mass fraction of 20:37:55), 4 parts of a suspension stabilizer, 3 parts of a retarder, 5 parts of a fluid loss additive, 1 part of a drag reducer, 1 part of a defoaming agent and 44 parts of water.
[0081] The preparation method is the same as that of Example 1.
[0082] Example 12
[0083] A 240°C ultra-high temperature resistant cementing slurry system of the present embodiment is prepared from the following raw material components in parts by weight: 100 parts of oil well G-grade cement, 1 part of a structural stabilizer (made from calcium carbonate whiskers and carbon fibers), 4 parts of a suspension stabilizer, 3 parts of a retarder, 5 parts of a fluid loss additive, 1 part of a drag reducer, 1 part of a defoaming agent, and 44 parts of water.
[0084] The preparation method is the same as that of Example 1.
[0085] Comparative Example 1
[0086] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 1 part of drag reducer, 1 part of defoamer, and 44 parts of water.
[0087] The preparation method is the same as that of Example 1.
[0088] Comparative Example 2
[0089] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 50 parts of 200-mesh ordinary quartz sand, 3 parts of retarder, 5 parts of fluid loss reducer, 3 parts of suspension stabilizer, 1 part of drag reducer, 1 part of defoamer, and 44 parts of water.
[0090] The preparation method is the same as that of Example 1.
[0091] Comparative Example 3
[0092] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 50 parts of 500-mesh ordinary quartz sand, 3 parts of retarder, 5 parts of fluid loss reducer, 3 parts of suspension stabilizer, 2 parts of drag reducer, 1 part of defoamer, and 44 parts of water.
[0093] The preparation method is the same as that of Example 1.
[0094] Comparative Example 4
[0095] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 25 parts of 200-mesh ordinary quartz sand, 25 parts of 500-mesh ordinary quartz sand, 3 parts of retarder, 5 parts of fluid loss reducer, 3 parts of suspension stabilizer, 1 part of drag reducer, 2 parts of defoamer, and 44 parts of water.
[0096] The preparation method is the same as that of Example 1.
[0097] Comparative Example 5
[0098] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 0.4 parts of carbon fiber, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 1 part of drag reducer, 1 part of defoamer, and 44 parts of water.
[0099] The preparation method is the same as that of Example 1.
[0100] Comparative Example 6
[0101] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 0.2 parts of carbon fiber, 1 part of calcium carbonate whisker, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 1 part of drag reducer, 1 part of defoamer, and 44 parts of water.
[0102] The preparation method is the same as that of Example 1.
[0103] Comparative Example 7
[0104] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 25 parts of 200-mesh ordinary quartz sand, 25 parts of 500-mesh ordinary quartz sand, 0.4 parts of carbon fiber, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 2 parts of drag reducer, 1 part of defoamer, and 44 parts of water.
[0105] The preparation method is the same as that of Example 1.
[0106] Comparative Example 8
[0107] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 25 parts of 200-mesh ordinary quartz sand, 25 parts of 500-mesh ordinary quartz sand, 0.2 parts of carbon fiber, 1 part of calcium carbonate whisker, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 2 parts of drag reducer, 1 part of defoamer, and 44 parts of water.
[0108] The preparation method is the same as that of Example 1.
[0109] Comparative Example 9
[0110] This comparative example is compared with comparative example 1, and the following raw materials are added in parts by weight: 100 parts of G-grade oil well cement, 25 parts of 200-mesh ordinary quartz sand, 25 parts of 500-mesh ordinary quartz sand, 0.2 parts of carbon fiber, 1 part of calcium carbonate whisker, 1 part of nano titanium dioxide, 3 parts of retarder, 5 parts of fluid loss additive, 3 parts of suspension stabilizer, 2 parts of drag reducer, 1 part of defoamer, and 44 parts of water.
[0111] The preparation method is the same as that of Example 1.
[0112] The cementing cement slurries of Examples 1 to 7 and Comparative Examples 1 to 9 were used as test objects. The solid dry ash component and the liquid water component of the cementing cement slurry system were weighed and mixed respectively. Then, the slurry was prepared according to the standard GB / T 19139-2012 "Test methods for oil well cement", and the performance of the cementing cement slurry system was tested with reference to the standard SY / T 6544-2017 "Performance requirements for oil well cement slurries".
[0113] Test Example 1: Test on the slurry performance of cement slurry resistant to ultra-high temperature of 240℃
[0114] The 240°C ultra-high temperature resistant cementing slurry of Examples 1 to 12 was used as the test object, and the cement slurry performance test was carried out for comparison with Comparative Examples 1 to 9. First, the solid dry ash component and the liquid water component of the 240°C ultra-high temperature resistant cementing slurry system were weighed and mixed, and then the slurry was prepared according to the standard GB / T 19139-2012 "Test method for oil well cement", and the performance of the cementing slurry system was tested with reference to the standard SY / T6544-2017 "Performance requirements for oil well cement slurry".
[0115] The test results are shown in Table 1. According to Table 1, the water loss of the 240°C ultra-high temperature cementing slurry prepared by the present invention is controlled within 50 mL, and has good rheological properties. The thickening time can also meet the relevant requirements of on-site cementing construction.
[0116] Table 1 Paste properties of different cement slurry systems
[0117]
[0118] Test Example 2: Mechanical properties test of cement slurry resistant to ultra-high temperature of 240℃
[0119] The ratios 1 to 9 of Examples 1 to 12 were cured in a high temperature and high pressure curing kettle for 7 days, 14 days, 28 days and 40 days respectively, and the compressive strength and elastic modulus of the cementing cement at different temperatures were tested using a uniform acceleration pressure testing machine. The relevant operation reference standards were the same as those of Test Example 1. The test results are shown in Table 2.
[0120] Table 2 Compressive strength and elastic modulus of different cement slurry systems
[0121]
[0122] Table 3 Compressive strength and elastic modulus of different cement slurry systems
[0123]
[0124] Table 4 Compressive strength and elastic modulus of different cement slurry systems
[0125]
[0126]
[0127] It can be seen from Table 2, Table 3 and Table 4 that the overall trend of comparative examples 1 to 9 is downward, which is specifically manifested in that the compressive strength of cement paste decreases with the increase of curing days, and the compressive strength decreases with the increase of temperature. Examples 1 to 12 show an overall trend of first rising and then falling, which is specifically manifested in that the compressive strength of cement paste reaches the maximum value when the curing days are 14 days, and the degree of hydration accelerates with the increase of temperature, the compressive strength of 7 days and 14 days increases with the increase of temperature, and the compressive strength of 28 days and 40 days decreases with the increase of temperature, and the compressive strength does not decline significantly with the increase of curing days. The single-addition experimental scheme examples 8 to 12 all improve the 7-day, 14-day, 28-day and 40-day compressive strength of cement paste to varying degrees. The cement slurry of Example 9, which only adds the strength stabilizer, shows a rapid increase in early compressive strength. This is because the strength stabilizer reacts with the hydration product calcium hydroxide to form hydrated calcium silicate, which improves the early compressive strength of cement paste. In Example 10, only the anti-strength decay agent was added. Due to the secondary hydration reaction with cement in the high-temperature hydrothermal environment, aluminum silicate was generated. The compressive strength of the cement stone increased rapidly, and there was no obvious decay in the compressive strength of the cement stone at 28 days and 40 days. In Example 11, only the lattice growth inhibitor was added. Due to the spatial resistance formed in the late hydration period, the formation of parallel needle-rod structures was prevented, and there was no obvious decay in the late compressive strength of the cement stone. In Example 12, only the structural stabilizer was added. Due to the bridging and pull-out effects of the inorganic single crystal material and the fiber material, the elastic modulus of the cement stone was lower, and the compressive strength was slightly improved compared with that of Comparative Example 1. Under the combined action of the four key additives, the compounded Example 1 had higher compressive strength and lower elastic modulus at each hydration stage.
[0128] Test Example 3: Effects of four key additives on the microstructure of cement paste
[0129] The cementing slurry systems of Example 1, Examples 4 to 7 and Comparative Examples 1 and 4 were used as test objects, and the porosity and permeability of the cementing slurry systems at different temperatures were tested by mercury intrusion and liquid permeability measurement, and the relevant operation reference standards were the same as those of Test Example 1. The specific experimental results are shown in Table 5.
[0130] Table 5 Porosity and permeability of different cement slurry systems
[0131]
[0132] According to the test results in Table 5, after the cement paste was cured for 40 days, the porosity and liquid permeability of the cement paste at 200°C, 220°C and 240°C were similar. Compared with Comparative Example 1, the porosity and permeability of Example 9, which only added the strength stabilizer, and Comparative Example 4, which added silica sand, did not change significantly, indicating that the effect of the volcanic ash reaction to generate hydrated calcium silicate on filling pores and reducing permeability was small. The porosity and permeability of the cement paste in Example 10, which added the anti-strength decay agent, were reduced. This is because the addition of the anti-strength decay agent optimized the pore size distribution of the cement paste, and the active ingredients in the anti-strength decay agent reacted with the cement hydration product to generate more hydration products, which could be filled in the pores of the cement paste, further increasing the porosity and permeability. The porosity and permeability of the cement paste in Example 11, which added the lattice growth inhibitor, were significantly reduced. In the early stage of hydration, the nanomaterials were filled in the voids of the cement paste, refining the harmful pores, and in the later stage, spatial resistance was formed to prevent the generation of loose structure hydration products, and the porosity was significantly reduced. The porosity and permeability of the cement paste of Example 12 with the addition of a structural stabilizer are slightly reduced compared to those of Comparative Example 1. This is because the whisker fiber material fills the pore space of the cement, eliminating the adverse effects of the pores and optimizing the pore size distribution. Figure 1 It can be seen that compared with Comparative Example 1, under the joint action of the crystal nucleus growth inhibitor, the structural stabilizer and the anti-strength decay agent, the microstructure of the composite example 1 is significantly denser. The reduction in porosity and permeability is manifested in the microstructure as a reduction in harmful voids and cracks, which has a positive effect on the improvement of the mechanical properties of cement paste, and is mutually verified with the substantial improvement in the compressive strength of Tables 2, 3 and 4.
[0133] Test Example 4: Effects of four key additives on hydration process
[0134] Figure 2 It is the hydration heat release rate curve of Example 1 and the blank control group comparative example 1 during the hydration process. The first exothermic peak is basically completed in the pre-induction period and induction period of cement slurry at 0 to 4 hours, and the peak value of Example 1 with added strength stabilizer is significantly higher than that of comparative example 3; the cement slurry hydration acceleration period is basically completed at 6 to 16 hours, and due to the effect of the anti-strength decay agent in Example 1, the exothermic rate peak value is higher and lasts longer; in the subsequent deceleration period and stabilization period, the peak values of the two groups of exothermic rate curves tend to be flat and gradually overlap. Figure 3 The cumulative heat release curves of hydration heat of the two groups of experiments are shown in FIG. 1 . Due to the promotion effect of the nanomaterials, the cumulative heat of Example 1 is higher than that of Comparative Example 1. The total heat release of the two groups is significantly different, which proves that more hydration products are generated.
[0135] In summary, the 240°C ultra-high temperature resistant cementing slurry system provided by the present invention can significantly improve the mechanical properties of cement stone, and the thickening time, rheological properties and API water loss of the cement slurry system of the present invention meet the relevant test requirements of cementing construction and have good application prospects.
[0136] The above is only a preferred specific implementation of the present invention, but the present invention is not limited to the examples listed. Similar effects can be obtained in other embodiments by using the relevant materials and the method mechanism in the present invention. Therefore, for those skilled in the art, without departing from the principles and spirit of the present invention, the improvements made are all within the scope of protection of the claims of the present invention.
Claims
1. A cement slurry system that can withstand ultra-high temperatures of 240°C. It is characterized in that The composition includes the following components by weight: 100 parts of oil well G grade cement, 30-50 parts of strength stabilizer, 5-15 parts of anti-strength decay agent, 0.3-1 parts of lattice growth inhibitor, 1-3 parts of structure stabilizer, 0.5-5 parts of suspension stabilizer, 0.5-5 parts of retarder, 4-10 parts of fluid loss reducer, 1-3 parts of drag reducer, 0.2-1 parts of defoamer and 38-60 parts of water; A 240°C ultra-high temperature resistant cementing slurry system, characterized in that specifically a strength stabilizer, an anti-strength decay agent, a lattice growth inhibitor and a structure stabilizer are added to the above-mentioned oil well cement; the strength stabilizer reduces the calcium-silicon ratio of the system, and reacts with the hydration product calcium hydroxide to generate more hydrated calcium silicate with good thermal stability and high strength, thereby improving the early compressive strength of the cement paste; under a high-temperature hydrothermal environment, the aluminum-containing minerals in the anti-strength decay agent react with the cement in the middle and late stages of hydration to generate a secondary cement hydration reaction, thereby inhibiting the generation of parallel needle-shaped structure hydration products and promoting the generation of high-temperature stable hydration products; the lattice growth inhibitor, as a nano-inert material, is filled in the cement paste. Certain defects are formed in the pores of the cement paste, providing crystallization points for the formation of hydration products, promoting early hydration reactions and increasing the density of cement paste, and forming spatial resistance in the middle and late stages of hydration to prevent the formation of fragile hydration products such as parallel needle-like structures; the micron material and fiber material in the structural stabilizer are evenly and anisotropically distributed on the micron scale to form a three-dimensional staggered hierarchical structure, delaying the formation of cracks in the process of cement paste being damaged; the composite action of the above four materials has a positive effect on the hydration products, crystal morphology, and stacking structure at different scales and different hydration stages, thereby controlling the cement hydration products, effectively regulating the microstructure of cement paste, and greatly improving the mechanical properties of oil well cement paste at high temperatures; The main component of the strength stabilizer is quartz sand, which can react with cement to produce pozzolanic reaction and reduce the calcium-silicon ratio of the cement system. The specific preparation process is as follows: the vein quartz is initially crushed into quartz particles of 50-80 meshes; concentrated hydrochloric acid with a mass fraction of 25-37% and hydrofluoric acid with a mass fraction of 5-20% and water with a volume ratio of 10-15:1-2:10-17 are mixed to prepare an acid solution, and the acid solution is acid-leached at room temperature for 10-12 hours and stirred at a speed of 100-150r / min; The impurities in the coarse ore particles are removed by water washing; a ball mill is used to grind the ore particles at a material-ball ratio of 1:2, a water ratio of 40-50%, and a ball milling time of 30-50 minutes, and then quartz sand with a particle size of 100-200 mesh is screened out as coarse quartz sand, and quartz sand with a particle size of 400-500 mesh is screened out as fine quartz sand, and the two quartz sands are mixed evenly at a mass fraction of 23-30:35-47 to obtain a strength stabilizer, which has the appearance of a white solid powder and a density of 2.65-2.70 g / cm 3 , purity is above 99.5%; The lattice growth inhibitor is mainly a nano-scale one-dimensional chemically inert material. On the one hand, it plays a physical filling role and fills in the micro-nano pores to increase the density of the cement paste; on the other hand, it plays a crystal nucleus role of the nano material, optimizes the nucleation site of the hydration product at low temperature, promotes the hydration reaction, and forms a spatial resistance at high temperature to prevent the transformation of the xonotlite crystal and the tobermorite crystal from the columnar structure to the parallel needle-rod structure; it is characterized in that the lattice growth inhibitor is obtained by uniformly mixing nano calcium carbonate, nano titanium dioxide and nano zirconium dioxide in a mass fraction of 20-43:15-37:25-55, wherein the particle size of the nano calcium carbonate is between 60-80nm, the particle size of the nano titanium dioxide is between 40-80nm, and the particle size of the nano zirconium dioxide is between 30-70nm; The anti-strength decay agent is mainly composed of aluminum-containing minerals, which can participate in secondary hydration reactions under high-temperature hydrothermal conditions, inhibit the formation of parallel needle-shaped structure hydration products, and generate high-temperature stable hydration products such as aluminum silicate; the anti-strength decay agent is obtained by uniformly mixing metakaolin, zeolite, bauxite and mullite in a mass fraction of 5 to 10:12 to 27:17 to 32:28 to 37, wherein the particle size of metakaolin is between 40 and 50 μm, the particle size of zeolite is between 75 and 106 μm, the particle size of bauxite is between 58 and 75 μm, and the particle size of mullite is between 48 and 75 μm; Among them, the structural stabilizer has the characteristics of large aspect ratio, high mechanical strength and high temperature resistance, can be bridged between the hydration products of oil well cement to build a three-dimensional staggered structure, and play the role of "pulling out" and "crack deflection". The specific preparation process of the crystal enhancer is to add 20 to 35 parts of inorganic single crystal material and 5 to 12 parts of fiber material in 100 parts of deionized water under stirring conditions of 200 to 300 rpm, and then add 8 to 15 parts of tetraethyl orthosilicate, adjust the pH to 5.0 to 6.0 with dilute hydrochloric acid, and then heat to 60 to 65°C, continue to react for 50 to 80 minutes under stirring, cool to room temperature, filter, and put into a 100 to 105°C oven for drying for 18 to 24 hours to obtain a crystal enhancer; characterized in that the inorganic single crystal material is one or a combination of calcium carbonate, aluminum borate and magnesium silicate inorganic single crystal materials, and the fiber material is one or a combination of carbon fiber and basalt fiber; A 240°C ultra-high temperature resistant cementing slurry system, characterized in that the fluid loss reducer is obtained by free radical copolymerization of N,N-dimethylacrylamide (NNDMA), 2-acrylamide-2-methylpropanesulfonic acid (AMPS), sodium styrene sulfonate (SSS) and itaconic acid (IA) in a mass fraction of 27-40:24-38:10-16:18-27 in pure water at 50-55°C through a sodium bisulfite-ammonium persulfate initiator system, wherein the reaction pH is 5.5-6.5 and the reaction time is 240-300 minutes; A 240°C ultra-high temperature resistant cementing slurry system, characterized in that the retarder is obtained by free radical copolymerization of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N,N-dimethylacrylamide (DMAA), acrylic acid (AA), and vinylphosphonic acid (VPA) in a mass fraction of 17-30:12-28:25-46:28-57 in pure water at 40-45°C with a hydrogen peroxide initiator, wherein the reaction pH is 3.0-3.5 and the reaction time is 360-480 minutes; A 240°C ultra-high temperature resistant cementing slurry system, characterized in that the suspension stabilizer is obtained by uniformly mixing solid powder of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), N,N-dimethylacrylamide (DMAA), and sodium styrene sulfonate (SSS) copolymer with nano-attapulgite and magnesium aluminum silicate in a mass fraction of 37-60:9-21:12-28.
2. A 240°C ultra-high temperature resistant cementing slurry system according to claim 1, It is characterized in that The drag reducer is one of sulfonated aldehyde ketone condensation drag reducers, naphthalene sulfonate drag reducers and polycarboxylic acid drag reducers, or a mixture thereof; the defoamer is one of phosphate defoamers, organosiloxane defoamers, organic polyether defoamers and organosilicon ether defoamers, or a mixture thereof; the oil well cement is G-grade oil well cement or H-grade oil well cement; and the water is fresh water or low-mineralized water.
Citation Information
Cited By
Cement system suitable for ultra-deep well cementation and preparation method thereof
CN119638290A
Preparation method and application of high-temperature cement stone strength decline inhibitor
CN121698598A
A method for preparing a high-temperature cement stone strength degradation inhibitor and its application
CN121698598B