Binder sol for nano ceramic tape casting slurry as well as preparation method and application of binder sol
By using binder sols of PVB, plasticizer and modifier in ceramic casting production, the problems of ceramic powder dispersion and colloid uniformity are solved, and casting slurry with high solids content and high performance are achieved , improves the strength and toughness of casting batches, simplifies the process and reduces costs.
Patent Information
- Application Number
- CN202411016455.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to achieve uniform dispersion of nanoparticle aluminum oxide and silicon carbide powder in ceramic casting production, resulting in uneven colloidal components in casting slurry, forming defects such as gels, bumps, hollows and cracks, and it is difficult to A cast slurry with high solids content and suitable performance is obtained.
Using a binder sol for nanoceramic casting slurry, including PVB, plasticizer and modifier, a stable colloid is formed through specific ratios and process methods, and used for ceramics such as nanoalumina and silicon carbide. The cast slurry of the powder ensures uniform dispersion and high solids content.
The uniform dispersion of nano-ceramic casting slurry is achieved, the strength and toughness of casting batches are improved, the preparation process is simplified, the cost is reduced, and the defects in casting production are avoided.
Smart Images

Figure BDA0004965857470000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrostatic chucks, and in particular to a binder sol for nano-ceramic casting slurry and a preparation method and application thereof. Background Art
[0002] Alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics have excellent high-temperature mechanical strength, high hardness, high elastic modulus, high wear resistance, high thermal conductivity, corrosion resistance, and excellent electrical insulation properties. They are widely used in the semiconductor field, such as chips and substrates.
[0003] The tape casting process is a method that can stably produce large batches of ceramic sheets. The ceramic tape casting film is required to have certain strength and toughness. It usually needs to use the role of polymer adhesives to evenly and densely bond the ceramic particles of the powder. Usually, acrylic resin (PMMA) and acetal resin (PVB) are commonly used as binders in the ceramic tape casting production process. PVB (polyvinyl butyral) is a synthetic resin produced by the reaction of polyvinyl alcohol and butyraldehyde, which has good adhesion, flexibility and chemical stability. PVB can swell in a non-polar / polar organic mixed solvent to form a stable colloid with a certain viscosity (CN 114752082A). The selected solvent has different affinity for the side chain groups of PVB according to its polarity and ratio, and exhibits different viscosities and fluidities. The stability and uniformity of the colloid are crucial to the quality of the tape casting slurry.
[0004] In the existing technical scheme: the key to preparing PVB sol is, first, to select PVB with suitable molecular weight and suitable functional group content according to the designed casting slurry, second, to select suitable non-polar / polar organic mixed solvent with a certain ratio, and third, to ensure that PVB is fully swollen in the solvent and can effectively adhere to the surface of ceramic powder particles to improve particle potential, pH, dispersibility, thixotropy, etc.; for casting slurries of different ceramic powders, it is necessary to design the sol formula and process in a special and targeted manner.
[0005] The shortcomings of the prior art are: for existing commercial ceramic powders such as nano-particle alumina and nano-particle silicon carbide, the surface morphologies of the two are very different, the chemical environment of the particle surface is complex, and it is difficult to evenly disperse the composite ceramic powders after a certain ratio; in addition, if the sol formed by PVB has a low degree of swelling, it will form micelles. The micelles are colloids with high PVB content that wrap the PVB that has not had time to dissolve in the middle. They cannot be completely removed by filtering, resulting in uneven colloid composition. The tape casting slurry made with this colloid as a raw material will form defects such as gel, bumps, voids, and cracks on the tape casting green batch; and for the need to obtain a slurry with a higher solid content and performance suitable for tape casting, higher requirements are placed on the stable sol formed by mixing a binder and a certain ratio of organic solvent. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a binder sol for nano-ceramic casting slurry and a preparation method and application thereof, so as to solve the problems raised in the background technology.
[0007] In order to solve the above technical problems, the technical solution of the present invention is:
[0008] On one hand, the present invention discloses a binder sol for nano-ceramic casting slurry, wherein the binder sol comprises: a binder PVB, a plasticizer, a solvent and a modifier, wherein the PVB binder accounts for 10wt.% to 25wt.% of the sol, the plasticizer accounts for 5wt.% to 15wt.% of the sol, and the modifier accounts for 0.5wt.% to 10wt.% of the sol.
[0009] Preferably, the molecular weight of the binder PVB is 30000-150000, the hydroxyl content of the binder PVB is 12wt.%-25wt.%, the acetoxy content is 1wt.%-4wt.%, the water content is lower than 2wt.%, and the glass transition temperature is 65°C-78°C.
[0010] Preferably, the plasticizer is any one of dibutyl phthalate (DBP), dioctyl phthalate (DOP), polyethylene glycol (PEG), or a mixture of two or more thereof.
[0011] Preferably, the solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene:alcohol:ketone to the sol is 3wt.%~12wt.%:2wt.%~6wt.%:0.4wt.%~2wt.%, and the solvent has a purity of more than 99.5% and a water content of less than 0.1wt.%.
[0012] Preferably, the modifier is a modified sol for better dispersion and coating of nano-sized silicon carbide SiC; the modifier is polyether-modified siloxane, fluorine-modified acrylic polymer, polyethylene glycol, n-octanol,
[0013] Another aspect of the present invention discloses a method for preparing a binder sol for nano-ceramic tape casting slurry, the method comprising:
[0014] S1: Weigh the following according to the proportion: binder PVB, plasticizer, solvent and modifier;
[0015] S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C to 50°C, and rotate at a speed that can evenly mix the solvents, which is 15 to 30 r / min;
[0016] S3: Add the adhesive PVB powder in step S1 into the constant temperature glue preparation barrel in step S2 in batches for multiple times, and increase the stirring speed in turn according to the amount of adhesive PVB powder added, with the maximum speed being 100 r / min;
[0017] S4: After the binder PVB is added, stir at a constant temperature for 0.5h to 2h;
[0018] S5: After the sol in step S4 is allowed to stand for 0.5 to 2 hours, it is filtered using a 300-mesh filter and then packaged into a fluorinated bottle for storage;
[0019] S6: adding alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramic slurries to the sol after standing in step S5 and performing ball milling dispersion to obtain a tape casting slurry.
[0020] The invention also discloses the application of a binder sol for nano ceramic tape casting slurry. The binder sol is applied to electronic grade nano alumina ceramics, silicon carbide ceramics and alumina-silicon carbide composite ceramic tape casting slurry.
[0021] Preferably, the preparation materials of the electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-alumina raw powder, the average grain size of the nano-alumina raw powder is 50nm to 1000nm, the specific surface area is 3m2 / g to 18m2 / g, and the particle shape is spherical particles.
[0022] Preferably, the preparation materials of the electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-grade silicon carbide raw powder, with an average grain size of 50nm to 600nm, a specific surface area of 10m2 / g to 25m2 / g, and spherical particles.
[0023] The above technical solution has the following beneficial effects:
[0024] The present invention provides a binder for electronic-grade nano-ceramic tape-casting slurry and a preparation method and application thereof, which matches the binder colloid used in the tape-casting process using existing commercial nano-grained alumina, nano-grained silicon carbide and other ceramic powders as raw materials, so as to obtain a tape-casting slurry with uniform dispersion and higher solid content. The preparation process of the colloid is simple, the raw material composition is less complex, the cost is low, and the prepared tape-casting green batch has high strength and good toughness. DETAILED DESCRIPTION
[0025] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0026] Example 1
[0027] The binder sol for nano-ceramic casting slurry comprises: binder PVB, plasticizer, solvent and modifier, wherein the PVB binder accounts for 10wt.% to 25wt.% of the sol, the plasticizer accounts for 5wt.% to 15wt.% of the sol, and the modifier accounts for 0.5wt.% to 10wt.% of the sol;
[0028] The molecular weight of the binder PVB is 30000-150000, preferably 40000-90000, the hydroxyl content of the binder PVB is 12wt.%-25wt.%, the hydroxyl content of the binder PVB is preferably 15wt.%-22wt.%, the acetoxy content is 1wt.%-4wt.%, the water content is less than 2wt.%, and the glass transition temperature is 65°C-78°C;
[0029] The plasticizer is any one of dibutyl phthalate (DBP), dioctyl phthalate (DOP), polyethylene glycol (PEG), or a mixture of two or more thereof;
[0030] The solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene: alcohol: ketone to the sol is 3wt.% to 12wt.%: 2wt.% to 6wt.%: 0.4wt.% to 2wt.%, the solvent has a purity of more than 99.5%, and the water content is less than 0.1wt.%;
[0031] The modifier is a modified sol for better dispersion and coating of nano-sized silicon carbide SiC; the modifier is polyether-modified siloxane, fluorine-modified acrylic polymer, polyethylene glycol, and n-octanol.
[0032] Example 2
[0033] The binder sol for nano-ceramic casting slurry comprises: a binder PVB, a plasticizer, a solvent and a modifier, wherein the PVB binder accounts for 10wt.% of the sol, the plasticizer accounts for 5wt.% of the sol, and the modifier accounts for 0.5wt.% of the sol;
[0034] The molecular weight of the binder PVB is 30000, the hydroxyl content of the binder PVB is 12wt.%, the acetoxy content is 1wt.%, the water content is less than 2wt.%, and the glass transition temperature is 65°C;
[0035] The plasticizer is any one of dibutyl phthalate (DBP), dioctyl phthalate (DOP), and polyethylene glycol (PEG);
[0036] The solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene: alcohol: ketone to the sol is 3wt.%: 2wt.%: 0.4wt.%, the purity of the solvent is above 99.5%, and the water content needs to be less than 0.1wt.%;
[0037] The modifier is mainly used to change the properties of the sol in order to better disperse and coat the nano-sized silicon carbide SiC; the modifier is polyether-modified siloxane, fluorine-modified acrylic polymer, polyethylene glycol, and n-octanol.
[0038] Example 3
[0039] The binder sol for nano-ceramic casting slurry comprises: a binder PVB, a plasticizer, a solvent and a modifier, wherein the PVB binder accounts for 25wt.% of the sol, the plasticizer accounts for 15wt.% of the sol, and the modifier accounts for 10wt.% of the sol;
[0040] The molecular weight of the binder PVB is 150000, the hydroxyl content of the binder PVB is 25wt.%, the acetoxy content is 4wt.%, the water content is 1.5wt.%, and the glass transition temperature is 78°C;
[0041] The plasticizer is a mixture of any two of dibutyl phthalate (DBP), dioctyl phthalate (DOP), and polyethylene glycol (PEG);
[0042] The solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene: alcohol: ketone to the sol is 12wt.%: 6wt.%: 2wt.%, the purity of the solvent is 99.7%, and the water content needs to be less than 0.1wt.%;
[0043] The modifier is a modified sol for better dispersion and coating of nano-sized silicon carbide SiC; the modifier is polyether-modified siloxane, fluorine-modified acrylic polymer, polyethylene glycol, and n-octanol.
[0044] Example 4
[0045] The binder sol for nano-ceramic casting slurry comprises: a binder PVB, a plasticizer, a solvent and a modifier, wherein the PVB binder accounts for 17wt.% of the sol, the plasticizer accounts for 10wt.% of the sol, and the modifier accounts for 2wt.% of the sol;
[0046] The molecular weight of the binder PVB is 90000, the hydroxyl content of the binder PVB is 18wt.%, the acetoxy content is 2wt.%, the water content is lower than 2wt.%, and the glass transition temperature is 71°C.
[0047] The plasticizer is a mixture of dibutyl phthalate (DBP), dioctyl phthalate (DOP) and polyethylene glycol (PEG).
[0048] The solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene: alcohol: ketone to the sol is 7wt. %: 4wt. %: 1wt. %, the solvent purity is 99.8%, and the water content is 0.05wt. %.
[0049] Example 5
[0050] A method for preparing a binder sol for nano-ceramic tape-casting slurry, the preparation method comprising:
[0051] S1: Weigh the following according to the proportion: binder PVB, plasticizer, solvent and modifier;
[0052] S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C to 50°C, and rotate at a speed that can evenly mix the solvents, which is 15 to 30 r / min;
[0053] S3: Add the adhesive PVB powder in step S1 into the constant temperature glue preparation barrel in step S2 in batches for multiple times, and increase the stirring speed in turn according to the amount of adhesive PVB powder added, with the maximum speed being 100 r / min;
[0054] S4: After the binder PVB is added, stir at a constant temperature for 0.5h to 2h;
[0055] S5: After the sol in step S4 is allowed to stand for 0.5 to 2 hours, it is filtered using a 300-mesh filter and then packaged into a fluorinated bottle for storage;
[0056] S6: adding alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramic slurries to the sol after standing in step S5 and performing ball milling dispersion to obtain a tape casting slurry.
[0057] Example 6
[0058] The method for preparing a binder sol for nano-ceramic tape casting slurry comprises:
[0059] S1: weigh the raw materials according to the ratio; the solvent is 200 parts of toluene, 100 parts of xylene, 100 parts of isopropanol, 30 parts of butanone, 55 parts of dibutyl phthalate (DBP) as a plasticizer, and 15 parts of a modifier is polyether-modified siloxane;
[0060] S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C to 50°C, preferably 35°C to 40°C, and rotate at a speed that can evenly mix the solvents, which is 15 to 30 r / min;
[0061] S3: adding the PVB powder in step S1 into the constant temperature glue preparation barrel in step 2 in batches for multiple times, and increasing the stirring speed in turn according to the amount of PVB powder added, with a maximum speed of 100 r / min;
[0062] S4: After PVB is added, stir at a constant temperature for 0.5h-2h;
[0063] S5: After the sol after step 4 is allowed to stand for 0.5-2 hours, it is filtered through a 300-mesh filter and then packaged into a fluorination bottle for storage.
[0064] Example 7
[0065] The method for preparing a binder sol for nano-ceramic tape casting slurry comprises:
[0066] S1: weigh the raw materials according to the ratio: 400 parts of toluene, 250 parts of isopropanol, 100 parts of butanone as solvent, 80 parts of dibutyl phthalate (DBP) as plasticizer, and 50 parts of polyethylene glycol as modifier;
[0067] S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C-50°C, preferably 35°C-40°C, and rotate at a speed that can evenly mix the solvents, which is 15-30 r / min;
[0068] S3: adding the PVB powder in step S1 into the constant temperature glue preparation barrel in step 2 in batches for multiple times, and increasing the stirring speed in turn according to the amount of PVB powder added, with a maximum speed of 100 r / min;
[0069] S4: After PVB is added, stir at a constant temperature for 0.5h to 2h;
[0070] S5: After the sol after step 4 is allowed to stand for 0.5 to 2 hours, it is filtered through a 300-mesh filter and then packaged into a fluorination bottle for storage.
[0071] Example 8
[0072] The method for preparing a binder sol for nano-ceramic tape casting slurry comprises:
[0073] S1: weigh the raw materials according to the ratio; the solvent is 150 parts of toluene, 100 parts of n-butanol, 50 parts of butanone, 60 parts of dibutyl phthalate (DBP) as a plasticizer, and 25 parts of a fluorine-modified acrylic polymer as a modifier;
[0074] S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C-50°C, preferably 35°C-40°C, and rotate at a speed that can evenly mix the solvents, which is 15-30 r / min;
[0075] S3: adding the PVB powder in step S1 into the constant temperature glue preparation barrel in step 2 in batches for multiple times, and increasing the stirring speed in turn according to the amount of PVB powder added, with a maximum speed of 100 r / min;
[0076] S4: After PVB is added, stir at a constant temperature for 0.5h to 2h;
[0077] S5: After the sol after step 4 is allowed to stand for 0.5 to 2 hours, it is filtered through a 300-mesh filter and then packaged into a fluorination bottle for storage.
[0078] The comparison of Example 6, Example 7 and Example 8 is shown in Table 1;
[0079] Table 1:
[0080]
[0081] Table 1 is a comparison of Example 6, Example 7, and Example 8. The corresponding viscosities are 2100 cP, 400 cPh, and 3800 cP, respectively. Four viscosity cups are shown in Table 1.
[0082] Example 9
[0083] Binder sol is used for electronic grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics tape casting slurry.
[0084] Among them, the preparation materials of electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-alumina raw powder, the average grain size of the nano-alumina raw powder is 50nm to 1000nm, preferably 100nm to 500nm, the specific surface area is 3m2 / g to 18m2 / g, preferably 5m2 / g to 12m2 / g, and the particle shape is spherical particles. In other embodiments of this embodiment, the average grain size of the nano-alumina raw powder is 50nm or 1000nm, and its specific surface area is 3m2 / g or 18m2 / g;
[0085] In other embodiments of the present embodiment, the preparation materials of electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-grade silicon carbide raw powder. The average grain size of the nano-grade silicon carbide raw powder is 50nm to 600nm, preferably 100nm to 300nm, and the specific surface area is 10m2 / g to 25m2 / g, preferably 12m2 / g to 20m2 / g. The particle shape is spherical particles. In other embodiments of the present embodiment, the average grain size of the nano-grade silicon carbide raw powder is 50nm or 600nm, and the specific surface area is 10m2 / g or 25m2 / g.
[0086] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A binder sol for nano-ceramic tape casting slurry, characterized in that: The binder sol comprises: binder PVB, plasticizer, solvent and modifier, wherein the PVB binder accounts for 10wt.% to 25wt.% of the sol, the plasticizer accounts for 5wt.% to 15wt.% of the sol, and the modifier accounts for 0.5wt.% to 10wt.% of the sol.
2. The binder sol for nano-ceramic tape casting slurry according to claim 1, characterized in that: The molecular weight of the binder PVB is 30000-150000, the hydroxyl content of the binder PVB is 12wt.%-25wt.%, the acetoxy content is 1wt.%-4wt.%, the water content is lower than 2wt.%, and the glass transition temperature is 65°C-78°C.
3. The binder sol for nano-ceramic tape casting slurry according to claim 1, characterized in that: The plasticizer is any one of dibutyl phthalate (DBP), dioctyl phthalate (DOP), and polyethylene glycol (PEG), or a mixture of two or more thereof.
4. The binder sol for nano-ceramic tape casting slurry according to claim 1, characterized in that: The solvent is a ternary solvent mixed with toluene, xylene, ethanol, propanol, isopropanol, n-butanol, isobutanol, sec-butanol and butanone, wherein the mass ratio of benzene: alcohol: ketone to the sol is 3wt.% to 12wt.%: 2wt.% to 6wt.%: 0.4wt.% to 2wt.%, and the solvent has a purity of more than 99.5% and a water content of less than 0.1wt.%.
5. The binder sol for nano-ceramic tape casting slurry according to claim 1, characterized in that: The modifier is a modified sol for better dispersion and coating of nano-sized silicon carbide SiC; the modifier is polyether-modified siloxane, fluorine-modified acrylic polymer, polyethylene glycol, and n-octanol.
6. A method for preparing a binder sol for nano-ceramic tape casting slurry as claimed in any one of claims 1 to 5, characterized in that: The method comprises: S1: Weigh the following according to the proportion: binder PVB, plasticizer, solvent and modifier; S2: First, pour the solvent, plasticizer and modifier in step S1 into a constant temperature plastic mixing barrel and stir slowly, keep the temperature at 30°C to 50°C, and rotate at a speed that can evenly mix the solvents, which is 15 to 30 r / min; S3: Add the adhesive PVB powder in step S1 into the constant temperature glue preparation barrel in step S2 in batches for multiple times, and increase the stirring speed in turn according to the amount of adhesive PVB powder added, with the maximum speed being 100 r / min; S4: After the binder PVB is added, stir at a constant temperature for 0.5h to 2h; S5: After the sol in step S4 is allowed to stand for 0.5 to 2 hours, it is filtered using a 300-mesh filter and then packaged into a fluorinated bottle for storage; S6: adding alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramic slurries to the sol after standing in step S5 and performing ball milling dispersion to obtain a tape casting slurry.
7. An application of the binder sol for nano-ceramic tape casting slurry as claimed in any one of claims 1 to 5, characterized in that: The binder sol is applied to binder sol for tape-casting slurry of electronic-grade nano-alumina ceramics, silicon carbide ceramics and alumina-silicon carbide composite ceramics.
8. The use of the binder sol for nano-ceramic tape casting slurry according to claim 7, characterized in that: The preparation materials of the electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-alumina raw powder, the average grain size of the nano-alumina raw powder is 50nm-1000nm, and the specific surface area is 3m 2 / g~18m 2 / g, the particle shape is spherical particles.
9. The use of the binder sol for nano-ceramic tape casting slurry according to claim 7, characterized in that: The preparation materials of the electronic-grade nano-alumina ceramics, silicon carbide ceramics, and alumina-silicon carbide composite ceramics include nano-scale silicon carbide raw powder, with an average grain size of 50nm to 600nm and a specific surface area of 10m 2 / g~25m 2 / g, the particle shape is spherical particles.
Citation Information
Patent Citations
Solvent system and preparation method and application thereof
CN114752082A
Preparation method for non-water-based high-purity nanoscale aluminum oxide ceramics
CN104987050A
Ceramic slurry, ceramic membrane tape and preparation method and application of ceramic slurry and ceramic membrane tape
CN114195487A
High-purity high-strength aluminum oxide ceramic substrate and preparation method thereof
CN115849885A
Cited By
A reversible temperature-sensitive suspension network alumina ceramic slurry and a preparation method thereof
CN122853857A