High-performance airtight concrete and preparation method thereof

By using low-heat cement, sulfoaluminate cement and nano SiO2 in vacuum pipeline systems, the hydration and hardening process of concrete is optimized, and the problem of insufficient sealing of concrete in vacuum pipeline systems is solved, and high-performance air-tight concrete is achieved The preparation of the product improves the sealing performance and gas permeability resistance and reduces construction costs.

CN119059780AActive Publication Date: 2024-12-03JIAHUA SPECIAL CEMENT

Patent Information

Application Number
CN202411107530.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing concrete materials are difficult to meet the high sealing requirements of vacuum pipeline systems in low vacuum environments, and the construction process is cumbersome, the steel structure welding workload is large, and there are problems such as difficult sealing performance.

Method used

Using low-heat cement, sulfur aluminate cement, predispersed nano SiO2 and characteristic admixtures, the particle accumulation density of powder and aggregate is enhanced by designing compaction, reducing internal pore size of the mixture, reducing defects, and optimizing the hydration and hardening of cement The process improves the compactness and crack resistance of concrete, and combines polycarboxylic acid high-performance water reducing agent and polyether defoaming agent to form high-performance airtight concrete.

Benefits of technology

It significantly improves the sealing performance and gas permeability of concrete in a vacuum environment, ensures low vacuum sealing of pipelines, reduces construction costs, and maintains the mechanical properties and airtightness of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991242200000061
    Figure BDA0004991242200000061
  • Figure BDA0004991242200000071
    Figure BDA0004991242200000071
  • Figure BDA0004991242200000111
    Figure BDA0004991242200000111
Patent Text Reader

Abstract

The invention discloses high-performance airtight concrete and a preparation method thereof. The concrete comprises 444-461 kg / m < 3 > of mixed cement; coal ash microspheres are 121-126 kg / m < 3 >; 162-168 kg / m < 3 > of mineral powder; 81-84 kg / m < 3 > of silica fume; the fine aggregate is 774-806 kg / m < 3 >; the coarse aggregate is 1114 to 1160kg / m < 3 >; 178-184 kg / m < 3 > of water; 2.02-2.1 kg / m < 3 > of a water reducing agent; 1.62 to 1.68 kg / m < 3 > of a defoaming agent; and the content of nano SiO2 is 28.08-16.76 kg / m < 3 > The low-heat cement is matched with the sulphoaluminate cement, the pre-dispersed nano SiO2 and the additive, so that the hydration and hardening process is improved, early and later compressive strength development and pore structure refinement of the concrete are facilitated, and the compactness and crack resistance of the concrete in a vacuum environment are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete materials, and in particular to high-performance airtight concrete and a preparation method thereof. Background Art

[0002] With the vigorous development of high-speed railways, people have put forward higher and higher requirements for the speed and convenience of transportation. As a new type of transportation system, the ultra-high-speed low-vacuum maglev pipeline system (referred to as the vacuum pipeline system) can effectively solve the resistance and noise problems generated by the operation of vehicles in an open air environment and improve the operating speed. In order to achieve the designed operating speed, the vacuum pipeline system must be able to establish and maintain low vacuum conditions inside, and the sealing performance of the pipeline structure itself and the connection parts is required to be high. At present, the vacuum pipeline system adopts the form of UN tube beam concrete structure wrapped with steel structure, that is, the upper N-shaped steel pipe and the lower U-shaped concrete wrapped steel plate are directly connected by welding to form a closed section to meet the low vacuum sealing performance; however, there are problems such as cumbersome construction process, large workload of steel structure welding, and difficulty in achieving high sealing performance of the tube beam. Therefore, it is necessary to explore a new type of high sealing performance material.

[0003] As the most economical and practical material, concrete can save economic costs if it is used as part of the vacuum piping system to replace the outer steel shell to achieve pipe-beam sealing. Relevant studies have shown that the airtightness of concrete is synonymous with the resistance to gas permeation, and is also the basic parameter for describing the durability process related to the migration of concrete and gas media. At present, scholars' research on airtight concrete is usually on ordinary concrete, which is mainly used in the construction of tunnels containing gas. In addition, concrete materials will aggravate the loss of internal water in a low vacuum environment, affect the hydration of concrete to a certain extent, and change the pore structure, which puts higher requirements on the airtightness of concrete. It can be seen that conventional concrete materials are difficult to meet the high sealing requirements of vacuum piping systems. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance airtight concrete and a preparation method thereof, which effectively reduces the internal pore size of the mixture by designing a high degree of particle packing density between the powder and the aggregate, and minimizes defects such as internal pores and microcracks; uses low-heat cement with low hydration heat, small water demand, good volume stability, and higher long-term strength, and is combined with sulphoaluminate cement, pre-dispersed nano-SiO 2 and special admixtures to improve the hydration and hardening process of cement, which is beneficial to the development of early and late compressive strength of concrete and refinement of pore structure, and improves the density and crack resistance of concrete in a vacuum environment, thereby meeting the low vacuum sealing of the pipeline.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] The invention discloses a high-performance airtight concrete, comprising the following raw materials per cubic meter of concrete: 444-461 kg / m of mixed cement; 3 ; Fly ash microbeads 121~126kg / m 3 ; Mineral powder 162~168kg / m 3 ; Silica fume 81~84kg / m 3 ; Fine aggregate 774~806kg / m 3 ; Coarse aggregate 1114~1160kg / m 3 ; Water 178~184kg / m 3 ; Water reducing agent 2.02~2.1kg / m 3 ; Defoamer 1.62~1.68kg / m 3 ; Nano-SiO 2 8.08~16.76kg / m 3 .

[0007] In some embodiments of the present invention, the mixed cement is a mixture of 42.5 grade low heat cement and 42.5 grade sulphoaluminate cement in a mass ratio of 6-10:0.5-1.2, preferably, in a mass ratio of 9.2:0.8.

[0008] In some embodiments of the present invention, the particle size of the fly ash microbeads is distributed between 0.5 and 4 μm, the particles are in a round glass shape, and the water demand ratio is 88%.

[0009] In some embodiments of the present invention, the specific surface area of ​​the mineral powder is 678m 2 / kg, and the activity index at 28 days was 105%.

[0010] In some embodiments of the present invention, the SiO 2 The content is greater than 93%, and the specific surface area is 23000m 2 / kg.

[0011] In some embodiments of the present invention, the fine aggregate is a well-graded zone II sand mixed with river sand with a particle size of 0 to 1.18 mm and machine-made sand with a particle size of 0 to 4.75 mm, and the river sand and machine-made sand are mixed in a mass ratio of 2:8; the apparent density of the fine aggregate is 2525 kg / m 3 , bulk density is 1710kg / m 3 , fineness modulus is 2.5, and mud content is 2.1%.

[0012] In some embodiments of the present invention, the coarse aggregate is a continuously graded crushed stone with a hard texture and a rough surface; the particle size of the coarse aggregate is distributed between 5 and 10 mm, the mud content is 0.7%, the crushing value is 5.2%, and the apparent density is 2782 kg / m 3 , bulk density is 1605kg / m 3 .

[0013] In some embodiments of the present invention, the water reducer is a polycarboxylic acid high-performance water reducer, a white powder, and a water reduction rate greater than 30%; the defoamer is a polyether defoamer, a light yellow powder, a viscosity of 800 to 1500 mPa·s, and a molecular weight of 3000 to 5000; the nano-SiO 2 The particle size is 30nm and the solid content is ≥99%.

[0014] The present invention discloses a method for preparing high-performance airtight concrete, comprising the following steps:

[0015] Step 1, preparing modified fly ash microbeads: adding HCl solution to fly ash microbeads, stirring and sealing, ultrasonically dispersing for 5 to 15 minutes, and then placing under magnetic stirring for reaction for 3 to 4 hours. After the stirring is completed, centrifugation and washing are performed rapidly until the pH of the supernatant is neutral, and then drying in a 70°C oven for 1.5 to 3 days to obtain modified fly ash microbeads;

[0016] Preferably, the mass percentage of fly ash microspheres to HCl solution is 15-20:80-85, and the concentration of HCl solution is 3 mol / L;

[0017] Modified fly ash microbeads can increase the surface roughness of fly ash and improve its adsorption capacity;

[0018] Step 2: Preparation of nano-SiO 2 — Fly ash microbead suspension: weigh nano-SiO 2 Set aside, and then weigh it as nano-SiO 2 The mass of modified fly ash microspheres is 1.5 to 2 times that of nano-SiO 2 The mass of water is 8 to 8.5 times that of nano-SiO 2 Add to water and disperse by ultrasonic for 3-8 minutes, then add modified fly ash microbeads and disperse by ultrasonic for 3-8 minutes to obtain nano-SiO 2 — Fly ash microsphere suspension;

[0019] Step 2 forms fly ash microbeads pre-dispersed nano-SiO 2 ;

[0020] Step 3: Weigh the mixed cement, fly ash microspheres, mineral powder, silica fume, fine aggregate, coarse aggregate, water, water reducer and defoamer according to the mass ratio for later use. The mass of the fly ash microspheres is the total mass of the fly ash microspheres minus the mass of the nano-SiO prepared in step 2. 2 —The mass of fly ash microspheres corresponding to the modified fly ash microspheres in the fly ash microsphere suspension, the mass of water is the total mass of water minus the mass of nano-SiO prepared in step 2 2 —The mass of water used in the fly ash microbead suspension;

[0021] Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material;

[0022] Step 5: Mix the water reducer and water weighed in step 3 and stir them thoroughly, then add the nano-SiO2 prepared in step 2. 2 —The fly ash microbead suspension is further stirred to obtain a mixture;

[0023] Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses nano-SiO 2 Pre-dispersion treatment is carried out to make it adsorbed on the surface of carrier particles (fly ash microbeads) and evenly dispersed in the concrete matrix, reducing its wrapping effect on cement particles. It can give full play to its nano-filling effect, chemical activity and nucleation effect, promote the cement hydration process, and optimize the interface transition zone structure; under the synergistic effect with the defoaming component, it also reduces the channels available for gas transmission and greatly reduces the gas permeability coefficient.

[0026] (2) The cement used in the present invention is low-heat cement and sulphoaluminate cement. Among them, low-heat cement has the characteristics of low water demand, low hydration heat, low shrinkage, high durability and excellent long-term mechanical properties. Using it as a cement material for airtight concrete can effectively improve the density and crack resistance of the concrete matrix while ensuring the working performance of the mixture, and enhance the sealing performance of the concrete; after being used with sulphoaluminate cement, the early strength and micro-expansion characteristics of sulphoaluminate cement can effectively make up for the low early strength of low-heat cement and further optimize the pore structure. Anhydrous calcium sulphoaluminate (CaA) in sulphoaluminate cement 3 When S) is hydrolyzed, nano-SiO 2 It can also preferentially adsorb Ca 2+ , promoting Ca 2+ and SO4 2- Diffusion, accelerating CaA 3 The hydrolysis of S provides more nucleation sites for the development of ettringite (AFt), making it easier for AFt to aggregate on the surface of cement particles, promoting early hydration, improving the interface transition zone, and making the internal structure of concrete denser.

[0027] (2) The high-performance airtight concrete of the present invention has good mechanical properties and anti-gas permeation performance, can effectively alleviate the chemical shrinkage caused by the loss of water inside the concrete under a vacuum environment, and enables the concrete to maintain excellent airtightness and volume stability after curing in a low vacuum environment, which can provide a reference for the track structure design of the vacuum pipeline system. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] In the embodiment of the present invention, the mixed cement is a mixture of 42.5 grade low heat cement and 42.5 grade sulphoaluminate cement in a mass ratio of 9.2:0.8.

[0030] In the embodiment of the present invention, the particle size of the fly ash microbeads is distributed between 0.5 and 4 μm, and the water requirement ratio is 88%.

[0031] In the embodiment of the present invention, the specific surface area of ​​the mineral powder is 678m 2 / kg, and the activity index at 28 days was 105%.

[0032] In the embodiment of the present invention, SiO 2 The content is greater than 93%, and the specific surface area is 23000m 2 / kg.

[0033] In the embodiment of the present invention, the fine aggregate is a zone II sand mixed with river sand with a particle size of 0 to 1.18 mm and machine-made sand with a particle size of 0 to 4.75 mm in a mass ratio of 2:8; the apparent density of the fine aggregate is 2525 kg / m 3 , bulk density is 1710kg / m 3 , fineness modulus is 2.5, and mud content is 2.1%.

[0034] In the embodiment of the present invention, the coarse aggregate is a continuously graded crushed stone; the particle size of the coarse aggregate is distributed between 5 and 10 mm, the mud content is 0.7%, the crushing value is 5.2%, and the apparent density is 2782 kg / m3 , bulk density is 1605kg / m 3 .

[0035] In the embodiment of the present invention, the water reducing agent is a polycarboxylic acid high-performance water reducing agent with a water reducing rate greater than 30%; the defoaming agent is a polyether defoaming agent with a viscosity of 800 to 1500 mPa·s and a molecular weight of 3000 to 5000; the nano-SiO 2 The particle size is 30nm and the solid content is ≥99%.

[0036] Example 1

[0037] As a preferred embodiment of the present invention, the high performance airtight concrete disclosed in this embodiment has a specific composition as shown in Table 1.

[0038] Table 1 Concrete ingredients for Example 1

[0039] Raw material name <![CDATA[Mass ratio kg / m 3 > cement 461 Fly ash microbeads 126 Mineral powder 168 Silica Fume 84 fine aggregate 774 coarse aggregate 1114 water 184 Water reducing agent 2.1 Defoaming agent 1.68 <![CDATA[Nano SiO 2 > 8.38

[0040] According to the mass ratio of each raw material in Table 1, the high-performance airtight concrete of this embodiment is prepared, including the following steps:

[0041] Step 1: Preparation of modified fly ash microspheres: fly ash microspheres (15.084 kg / m 3 ) was added with HCl solution, the mass percentage of fly ash microbeads and HCl solution was 16:84, the concentration of HCl solution was 3 mol / L, the mixture was stirred with a glass rod and then sealed, placed in an ultrasonic disperser for ultrasonic dispersion for 10 min, and then placed in a magnetic stirrer for magnetic stirring for 4 h. After the stirring was completed, the mixture was quickly centrifuged and washed until the pH of the supernatant was neutral, and then placed in a 70° C. oven for drying for 2 d to obtain modified fly ash microbeads;

[0042] Step 2: Preparation of nano-SiO 2 — Fly ash microsphere suspension: weigh 8.38kg / m 3 Nano-SiO 2 Set aside, and then weigh it as nano-SiO 2 The mass of modified fly ash microspheres is 1.8 times (15.084kg / m 3 ) and nano-SiO 2 The mass of water is 8.3 times (69.554 kg / m 3 ), the nano-SiO 2 Add water and disperse by ultrasonic for 5 min, then add modified fly ash microbeads and disperse by ultrasonic for 5 min to obtain nano-SiO 2 — Fly ash microsphere suspension;

[0043] Step 3: Weigh cement (461kg / m 3), fly ash microbeads ((126-15.084=110.916) kg / m 3 ), mineral powder (168kg / m 3 )、Silica fume (84kg / m 3 )、fine aggregate (774kg / m 3 ), coarse aggregate (1114kg / m 3 ), water ((184-69.554=114.446) kg / m 3 )、Water reducing agent (2.1kg / m 3 ) and defoamer (1.68kg / m 3 )spare;

[0044] Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material;

[0045] Step 5: Mix the water reducer and water weighed in step 3 and stir them thoroughly, then add the nano-SiO2 prepared in step 2. 2 —The fly ash microbead suspension is further stirred to obtain a mixture;

[0046] Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

[0047] Example 2

[0048] As a preferred embodiment of the present invention, the high performance airtight concrete disclosed in this embodiment has a specific composition as shown in Table 2.

[0049] Table 2 Concrete ingredients for Example 2

[0050]

[0051]

[0052] According to the mass ratio of each raw material in Table 2, the high-performance airtight concrete of this embodiment is prepared, including the following steps:

[0053] Step 1: Preparation of modified fly ash microspheres: fly ash microspheres (30.168 kg / m 3) was added with HCl solution, the mass percentage of fly ash microbeads and HCl solution was 16:84, the concentration of HCl solution was 3 mol / L, the mixture was stirred with a glass rod and then sealed, placed in an ultrasonic disperser for ultrasonic dispersion for 10 min, and then placed in a magnetic stirrer for magnetic stirring for 4 h. After the stirring was completed, the mixture was quickly centrifuged and washed until the pH of the supernatant was neutral, and then placed in a 70° C. oven for drying for 2 d to obtain modified fly ash microbeads;

[0054] Step 2: Preparation of nano-SiO 2 — Fly ash microsphere suspension: weigh 16.76 kg / m 3 Nano-SiO 2 Set aside, and then weigh it as nano-SiO 2 Modified fly ash microspheres with a mass 1.8 times that of the original (30.168 kg / m 3 ) and nano-SiO 2 8.3 times the mass of water (139.108 kg / m 3 ), the nano-SiO 2 Add water and disperse by ultrasonic for 5 minutes, then add modified fly ash microbeads and disperse by ultrasonic for 5 minutes to obtain nano-SiO 2 — Fly ash microsphere suspension;

[0055] Step 3: Weigh cement (461kg / m 3 ), fly ash microbeads ((126-30.168=95.832)kg / m 3 ), mineral powder (168kg / m 3 )、Silica fume (84kg / m 3 )、fine aggregate (774kg / m 3 ), coarse aggregate (1114kg / m 3 ), water ((184-139.108=44.892) kg / m 3 )、Water reducing agent (2.1kg / m 3 ) and defoamer (1.68kg / m 3 )spare;

[0056] Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material;

[0057] Step 5: Mix the water reducer and water weighed in step 3 and stir them thoroughly, then add the nano-SiO2 prepared in step 2. 2 —The fly ash microbead suspension is further stirred to obtain a mixture;

[0058] Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

[0059] Example 3

[0060] As a preferred embodiment of the present invention, the high performance airtight concrete disclosed in this embodiment has a specific composition as shown in Table 3.

[0061] Table 3 Concrete ingredients for Example 3

[0062] Raw material name <![CDATA[Mass ratio kg / m 3 > cement 444 Fly ash microbeads 121 Mineral powder 162 Silica Fume 81 fine aggregate 806 coarse aggregate 1160 water 178 Water reducing agent 2.02 Defoaming agent 1.62 <![CDATA[Nano - SiO 2 > 8.08

[0063] According to the mass ratio of each raw material in Table 3, the high-performance airtight concrete of this embodiment is prepared, including the following steps:

[0064] Step 1: Preparation of modified fly ash microspheres: 3 ) was added with HCl solution, the mass percentage of fly ash microbeads and HCl solution was 16:84, the concentration of HCl solution was 3 mol / L, the mixture was stirred with a glass rod and then sealed, placed in an ultrasonic disperser for ultrasonic dispersion for 10 min, and then placed in a magnetic stirrer for magnetic stirring for 4 h. After the stirring was completed, the mixture was quickly centrifuged and washed until the pH of the supernatant was neutral, and then placed in a 70° C. oven for drying for 2 d to obtain modified fly ash microbeads;

[0065] Step 2: Preparation of nano-SiO 2 — Fly ash microsphere suspension: weigh 8.08kg / m 3 Nano-SiO 2 Set aside, and then weigh it as nano-SiO 2 The mass of modified fly ash microspheres is 1.8 times (14.544kg / m 3 ) and nano-SiO 2 The mass of water is 8.3 times (67.064 kg / m 3 ), the nano-SiO 2 Add water and disperse by ultrasonic for 5 minutes, then add modified fly ash microbeads and disperse by ultrasonic for 5 minutes to obtain nano-SiO 2 — Fly ash microsphere suspension;

[0066] Step 3: Weigh cement (444kg / m 3 ), fly ash microbeads ((121-14.544=106.456) kg / m 3 ), mineral powder (162kg / m 3 ), silica fume (81kg / m 3 ), fine aggregate (806kg / m 3 ), coarse aggregate (1160kg / m3 ), water ((178-67.064=110.936) kg / m 3 )、Water reducing agent (2.02kg / m 3 ) and defoamer (1.62kg / m 3 )spare;

[0067] Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material;

[0068] Step 5: Mix the water reducer and water weighed in step 3 and stir them thoroughly, then add the nano-SiO2 prepared in step 2. 2 —The fly ash microbead suspension is further stirred to obtain a mixture;

[0069] Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

[0070] Example 4

[0071] As a preferred embodiment of the present invention, the high performance airtight concrete disclosed in this embodiment has a specific composition as shown in Table 4.

[0072] Table 4 Concrete ingredients list for Example 4

[0073] Raw material name <![CDATA[Mass ratio kg / m 3 > cement 444 Fly ash microbeads 121 Mineral powder 162 Silica Fume 81 fine aggregate 806 coarse aggregate 1160 water 178 Water reducing agent 2.02 Defoaming agent 1.62 <![CDATA[Nano SiO 2 > 16.16

[0074] According to the mass ratio of each raw material in Table 4, the high-performance airtight concrete of this embodiment is prepared, including the following steps:

[0075] Step 1: Preparation of modified fly ash microspheres: 3 ) was added with HCl solution, the mass percentage of fly ash microbeads and HCl solution was 16:84, the concentration of HCl solution was 3 mol / L, the mixture was stirred with a glass rod and then sealed, placed in an ultrasonic disperser for ultrasonic dispersion for 10 min, and then placed in a magnetic stirrer for magnetic stirring for 4 h. After the stirring was completed, the mixture was quickly centrifuged and washed until the pH of the supernatant was neutral, and then placed in a 70° C. oven for drying for 2 d to obtain modified fly ash microbeads;

[0076] Step 2: Preparation of nano-SiO 2 — Fly ash microsphere suspension: weigh 16.16 kg / m 3 Nano-SiO 2 Set aside, and then weigh it as nano-SiO 2 The mass of modified fly ash microspheres is 1.8 times that of the 3) and nano-SiO 2 The mass of water is 8.3 times (134.128 kg / m 3 ), the nano-SiO 2 Add water and disperse by ultrasonic for 5 min, then add modified fly ash microbeads and disperse by ultrasonic for 5 min to obtain nano-SiO 2 — Fly ash microsphere suspension;

[0077] Step 3: Weigh cement (444kg / m 3 ), fly ash microbeads ((121-29.088=91.912)kg / m 3 ), mineral powder (162kg / m 3 ), silica fume (81kg / m 3 ), fine aggregate (806kg / m 3 ), coarse aggregate (1160kg / m 3 ), water ((178-134.128=43.872) kg / m 3 )、Water reducing agent (2.02kg / m 3 ) and defoamer (1.62kg / m 3 )spare;

[0078] Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material;

[0079] Step 5: Mix the water reducer and water weighed in step 3 and stir them thoroughly, then add the nano-SiO2 prepared in step 2. 2 —The fly ash microbead suspension is further stirred to obtain a mixture;

[0080] Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

[0081] Comparative Example 1

[0082] The concrete for this comparison is the same as that of Example 1 except that ordinary Portland cement (PO42.5 cement) is used instead of mixed cement.

[0083] Comparative Example 2

[0084] The concrete for this comparison is the same as that of Example 2 except that ordinary Portland cement (PO42.5 cement) is used instead of mixed cement.

[0085] Comparative Example 3

[0086] The concrete for this comparison is the same as that of Example 3 except that ordinary Portland cement (PO42.5 cement) is used instead of mixed cement.

[0087] Comparative Example 4

[0088] The concrete for this comparison is the same as that of Example 4 except that ordinary Portland cement (PO42.5 cement) is used instead of mixed cement.

[0089] Comparative Example 5

[0090] The concrete in this comparison, except for the addition of nano-SiO 2 — Fly ash microsphere suspension and nano-SiO 2 Except for this, the rest are the same as in Example 1.

[0091] Comparative Example 6

[0092] The concrete in this comparison, except for the addition of nano-SiO 2 — Fly ash microsphere suspension and nano-SiO 2 Except for this, the rest are the same as in Example 3.

[0093] Comparative Example 7

[0094] In addition to adding nano-SiO 2 (i.e. without preparing and adding nano-SiO 2 —fly ash microbead suspension), the rest are the same as in Example 4.

[0095] Test Case

[0096] The concrete of Examples 1 to 4 and Comparative Examples 1 to 4 were cured, and the curing method was as follows: the concrete was subjected to standard curing for 28 days according to GB / T50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". After the curing was completed, some specimens were tested; some specimens were tested after continuing standard curing for 28 days; and the other specimens were moved into a vacuum curing box and tested after continuing curing for 28 days under an environment of 10,000 Pa.

[0097] After the test blocks used in the gas permeability test reach the corresponding curing age, they must refer to the standard JC / T2758-2023 "Test Method for Gas Permeability of Concrete" and carry out the test after the test blocks are cut, sealed and dried.

[0098] (1) Compressive strength test: According to GB / T50081-2019 Standard for Test Methods for Mechanical Properties of Ordinary Concrete, compressive strength tests were carried out on concrete specimens under different curing conditions.

[0099] (2) Gas permeability test: According to JC / T2758-2023 "Test method for gas permeability of concrete", gas permeability tests were carried out on concrete specimens under different curing conditions. A cylindrical concrete specimen with a diameter of 150 mm and a height of 50 mm was used, and the test gas path pressure was selected to be 0.8 MPa.

[0100] The test results are shown in Table 5.

[0101] Table 5 Test data

[0102]

[0103]

[0104] (1) As shown in Table 5, by comparing Examples 1-4, it can be found that under different curing methods, the concrete within each component range has good mechanical properties and gas permeation resistance; and after 28 days of vacuum curing, the overall performance of the specimen is still improving, but it is significantly lower than the concrete specimen after 56 days of standard curing.

[0105] (2) As shown in Table 5, by comparing Examples 1-4 with Comparative Examples 1-4, it can be found that under different curing methods and ages, the overall performance of the concrete using the mixed cement is better than that of the ordinary Portland cement group, especially under long-term curing, the low-heat cement can significantly improve the compressive strength and air tightness of the concrete; after 56 days of standard curing, the overall performance of Example 2 is the best, with a compressive strength of 133.7 MPa and a gas permeability coefficient of 0.01×10 -18 m 2 . Due to the loss of water inside the concrete under vacuum curing, the hydration rate is reduced and the pore structure is changed; by comparison, it is found that the gas permeability coefficient of comparative examples 1-4 is not much reduced compared with the standard curing for 28 days, and some groups have increased, while this phenomenon does not occur in the embodiment, which shows that the concrete prepared by low-heat cement has better adaptability to the vacuum environment and better airtightness performance.

[0106] (3) As shown in Table 5, by comparing Examples 1, 2 and Comparative Example 5, Examples 3, 4 and Comparative Example 6, it can be found that under different curing methods, the nano-SiO 2 —The addition of fly ash microbead suspension greatly improves the compressive strength and gas permeation resistance of the matrix, and the performance increases with the increase of the dosage. This is because the nano-SiO 2 Adsorption on the surface of fly ash microbeads improves the 2 The dispersion of nano-SiO 2It can better exert its nano-filling effect, chemical activity, crystal nucleation effect and optimize the structure of the interface transition zone. In synergistic effect with the defoaming component, it reduces the channels available for gas transmission and significantly reduces the gas permeability coefficient.

[0107] (4) As shown in Table 5, by comparing Example 4 with Comparative Example 7, compared with directly adding nano-SiO 2 , the nano-SiO 2 The particles are wrapped on the carrier material and act on the concrete to increase the SiO 2 Dispersibility reduces its wrapping effect on cement, promotes cement hydration process, is beneficial to increase the compressive strength of the matrix in the later stage and refine the pore structure, and improves the concrete's anti-gas permeability performance.

[0108] In summary, the high-performance airtight concrete prepared by the present invention is prepared by pre-dispersing nano-SiO 2 The synergistic effect improves the internal pore structure of concrete, reduces the gas permeability of concrete, and improves the durability of concrete. In addition, the combination of low-heat cement and sulphoaluminate cement can significantly optimize the workability and working stability of concrete, improve the dispersion stability of mineral admixtures and additives, effectively improve the density and crack resistance of concrete matrix, and enhance the sealing performance of concrete, so that concrete can still maintain excellent mechanical properties and air tightness in a vacuum environment.

[0109] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A high-performance airtight concrete, characterized in that: Includes the following raw materials per cubic meter of concrete: mixed cement 444~461kg / m 3 ; Fly ash microbeads 121~126kg / m 3 ; Mineral powder 162~168kg / m 3 ; Silica fume 81~84kg / m 3 ; Fine aggregate 774~806kg / m 3 ; Coarse aggregate 1114~1160kg / m 3 ; Water 178~184kg / m 3 ; Water reducing agent 2.02~2.1kg / m 3 ; Defoamer 1.62~1.68kg / m 3 ;Nano-SiO28.08~16.76kg / m 3 .

2. The high performance airtight concrete according to claim 1, characterized in that: The mixed cement is a mixture of 42.5-grade low-heat cement and 42.5-grade sulphoaluminate cement in a mass ratio of 6-10:0.5-1.2, preferably, in a mass ratio of 9.2:0.

8.

3. The high performance airtight concrete according to claim 1, characterized in that: The particle size of the fly ash microbeads is distributed between 0.5 and 4 μm, and the water requirement ratio is 88%.

4. The high performance airtight concrete according to claim 1, characterized in that: The specific surface area of ​​the mineral powder is 678m 2 / kg, and the activity index at 28 days was 105%.

5. The high performance airtight concrete according to claim 1, characterized in that: The SiO2 content in the silica ash is greater than 93%, and the specific surface area is 23000m 2 / kg.

6. The high performance airtight concrete according to claim 1, characterized in that: The fine aggregate is zone II sand mixed with river sand with a particle size of 0-1.18 mm and machine-made sand with a particle size of 0-4.75 mm. The river sand and machine-made sand are mixed in a mass ratio of 2:

8. The apparent density of the fine aggregate is 2525 kg / m 3 , bulk density is 1710kg / m 3 , fineness modulus is 2.5, and mud content is 2.1%.

7. The high performance airtight concrete according to claim 1, characterized in that: The coarse aggregate is a continuously graded crushed stone; the particle size of the coarse aggregate is distributed between 5 and 10 mm, the mud content is 0.7%, the crushing value is 5.2%, and the apparent density is 2782 kg / m 3 , bulk density is 1605kg / m 3 .

8. The high performance airtight concrete according to claim 1, characterized in that: The water reducer is a polycarboxylic acid high-performance water reducer with a water reduction rate greater than 30%; the defoamer is a polyether defoamer with a viscosity of 800-1500mPa·s and a molecular weight of 3000-5000; the particle size of the nano-SiO2 is 30nm and the solid content is ≥99%.

9. A method for preparing high-performance airtight concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1, preparing modified fly ash microbeads: adding HCl solution to fly ash microbeads, stirring and sealing, ultrasonically dispersing for 5 to 15 minutes, and then placing under magnetic stirring for reaction for 3 to 4 hours. After the stirring is completed, centrifugation and washing are performed rapidly until the pH of the supernatant is neutral, and then drying in a 70°C oven for 1.5 to 3 days to obtain modified fly ash microbeads; Preferably, the mass percentage of fly ash microspheres to HCl solution is 15-20:80-85, and the concentration of HCl solution is 3 mol / L; Step 2, preparing a nano-SiO2-fly ash microbead suspension: weigh nano-SiO2 according to the mass ratio for use, then weigh modified fly ash microbeads 1.5 to 2 times the mass of nano-SiO2 and water 8 to 8.5 times the mass of nano-SiO2, add nano-SiO2 into water and ultrasonically disperse for 3 to 8 minutes, then add modified fly ash microbeads and ultrasonically disperse for 3 to 8 minutes to obtain a nano-SiO2-fly ash microbead suspension; Step 3, respectively weigh the mixed cement, fly ash microspheres, mineral powder, silica fume, fine aggregate, coarse aggregate, water, water reducer and defoamer according to the mass ratio for use, wherein the mass of the fly ash microspheres is the total mass of the fly ash microspheres minus the mass of the fly ash microspheres corresponding to the modified fly ash microspheres in the nano-SiO2-fly ash microsphere suspension prepared in step 2, and the mass of water is the total mass of water minus the mass of water in the nano-SiO2-fly ash microsphere suspension prepared in step 2; Step 4: Mix the mixed cement, fly ash microbeads, mineral powder, silica fume and defoamer weighed in step 3 evenly; then add the weighed coarse aggregate and fine aggregate and continue to stir to obtain a mixed dry material; Step 5, the water reducing agent and water weighed in step 3 are fully mixed and stirred, and then the nano-SiO2-fly ash microbead suspension prepared in step 2 is added and stirred to obtain a mixture; Step 6: Pour the mixture into a mold, vibrate it to compact it, and then cover it with a film for curing in an environment of 18°C ​​to 22°C. After it is formed and hardened, high-performance airtight concrete is obtained.

Citation Information

Patent Citations

  • Nano-micron composite concrete powder early strength agent and preparation method thereof

    CN113121143A

  • High-airtightness concrete and preparation method thereof

    CN114573288A

Cited By

  • Low-shrinkage high-airtightness concrete and preparation method thereof

    CN119797861A

  • Low-shrinkage high-airtightness concrete and preparation method thereof

    CN119797861B

  • Special cementing material for low-shrinkage high-airtightness concrete and preparation method of special cementing material

    CN119797862A

  • A low-shrinkage high-airtightness concrete special binding material and a preparation method thereof

    CN119797862B