A precise production system and method for electrolytic copper foil
By using electrolytic copper foil precision production system and methods in electrolytic copper foil production, the current intensity and time are adjusted in real time, the production error problems caused by fixed current efficiency and parameters in the existing technology are solved, and higher production accuracy is achieved and flexibility.
Patent Information
- Application Number
- CN202310436794.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-21
AI Technical Summary
In the existing electrolytic copper foil production technology, fixed current efficiency values and parameters lead to large production errors and cannot meet the requirements of accurate production.
The electrolytic copper foil precision production system and method are adopted to obtain the target current efficiency value and production specifications through the production control module, calculate the initial electrolysis time and current intensity based on the preset electrolysis model, and adjust the current intensity and time in real time during the production process to achieve accurate results. control.
Improves production flexibility and accuracy, reduces product errors, and achieves more accurate copper foil production.
Smart Images

Figure CN116463691B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic foil manufacturing, and in particular to a precise production method of electrolytic copper foil. Background Art
[0002] With the development of science and technology, the demand for metal foil in all walks of life is also increasing. Electrolysis is the most common production method of metal foil. The metal foil obtained by this method has a wide range of uses, such as copper foil, aluminum foil, nickel foil, iron foil, etc.
[0003] At present, in the field of electrolytic copper foil, there are many factors that affect the quality and quantity of the final product, such as the current efficiency value and electrolysis time during the electrolysis process. In the prior art, a fixed current efficiency value is generally used for calculation and fixed parameters are used for production, which often leads to a large error in the final production. Although it is possible to adjust certain parameters during the production process to achieve the purpose of regulating the production results, the current solution still cannot achieve the desired level of accuracy.
[0004] Therefore, people are in urgent need of a new process solution for the production of electrolytic copper foil to achieve the purpose of precise production. Summary of the invention
[0005] In view of this, it is necessary to provide an electrolytic copper foil precision production system and an electrolytic copper foil precision production method to achieve the purpose of precision production of copper foil.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides an electrolytic copper foil precision production system, comprising a production execution mechanism and a production control module, wherein the production execution mechanism is used to electrolyze to obtain copper foil, the production execution mechanism is electrically connected to the production control module, and the production control module comprises an efficiency value determination module, an initial parameter calculation module, a production start module and a production adjustment module which are electrically connected in sequence, wherein:
[0008] The efficiency value determination module is used to obtain a target current efficiency value;
[0009] The initial parameter calculation module is used to obtain the target production specifications, and according to the target production specifications, based on the preset electrolysis model and the target current efficiency value, obtain the initial electrolysis time and the initial current intensity;
[0010] The production start module is used to send a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity, so as to control the production execution mechanism to start electrolysis;
[0011] The production adjustment module is used to obtain actual production specifications, and according to the actual production specifications and the target production specifications, based on the preset electrolysis model, obtain a corrected current intensity, and send a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0012] Furthermore, the production execution mechanism also includes a motor, a reduction transmission mechanism, a cathode roller and an electrolytic cell, the motor is transmission-connected to the reduction transmission mechanism, the reduction transmission mechanism is transmission-connected to the cathode roller, and the circumferential surface of the cathode roller extends into the electrolytic cell.
[0013] In a second aspect, the present invention further provides a method for accurately producing electrolytic copper foil, which is applied to the above-mentioned accurate production system for electrolytic copper foil, comprising:
[0014] Obtaining a target current efficiency value;
[0015] Obtaining target production specifications, and obtaining an initial electrolysis time and an initial current intensity according to the target production specifications, based on a preset electrolysis model and the target current efficiency value;
[0016] Sending a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity to control the production execution mechanism to start electrolysis;
[0017] The actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and a signal is sent to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0018] Further, the actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and according to the corrected current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis, including:
[0019] Obtaining a first production deviation value according to the actual production specification and the target production specification;
[0020] According to the first production deviation value and based on the preset electrolysis model, the initial current intensity is corrected to obtain the corrected current intensity;
[0021] A signal is sent to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0022] Furthermore, before obtaining the actual production specifications, obtaining the corrected current intensity based on the preset electrolysis model according to the actual production specifications and the target production specifications, and sending a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis, it also includes:
[0023] The actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected electrolysis time is obtained, and a signal is sent to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
[0024] Further, the actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected electrolysis time is obtained, and according to the corrected electrolysis time, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis, including:
[0025] Obtaining a second production deviation value according to the actual production specification and the target production specification;
[0026] According to the second production deviation value and based on the preset electrolysis model, the initial electrolysis time is corrected to obtain the corrected electrolysis time;
[0027] A signal is sent to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
[0028] Further, sending a signal to the production execution mechanism according to the modified electrolysis time to control the production execution mechanism to continue electrolysis includes:
[0029] Obtaining cathode roller specification parameters of the cathode roller;
[0030] According to the cathode roller specification parameters and the corrected electrolysis time, a target cathode roller rotation speed is obtained;
[0031] According to the target cathode roller rotation speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
[0032] Further, sending a signal to the production execution mechanism according to the target cathode roller speed to control the production execution mechanism to continue electrolysis includes:
[0033] Obtaining motor specification parameters of the motor and transmission specification parameters of the reduction transmission mechanism;
[0034] Obtaining a target motor speed according to the motor specification parameters, the transmission specification parameters and the target cathode roller speed;
[0035] According to the target motor speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
[0036] Furthermore, the preset electrolysis model includes:
[0037] M=KITη
[0038] Wherein M is the production specification, K is the electrochemical equivalent, I is the current intensity, T is the electrolysis time, and η is the current efficiency value.
[0039] Further, the obtaining of the target current efficiency value includes:
[0040] Sending a signal to the production execution mechanism to conduct trial production, and obtaining trial production product parameters and actual mechanism state parameters of the production execution mechanism;
[0041] According to the actual mechanism state parameters, an initial current efficiency value is obtained;
[0042] The initial current efficiency value is corrected according to the trial production product parameters to obtain the target current efficiency value.
[0043] The present invention provides an electrolytic copper foil precision production system and an electrolytic copper foil precision production method, wherein the system includes a production execution mechanism and a production control module. During production, a target current efficiency value is first obtained, and then a target production specification is obtained. According to the target production specification, based on a preset electrolysis model and the target current efficiency value, an initial electrolysis time and an initial current intensity are obtained. Then, according to the initial electrolysis time and the initial current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to start electrolysis. Finally, the actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and according to the corrected current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis. Compared with the prior art, the present invention does not use fixed parameters for production, but uses non-fixed current, and adjusts to the corrected current intensity at any time during the production process, so that the production is flexible and more accurate. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 A system architecture diagram of an embodiment of an electrolytic copper foil precision production system provided by the present invention;
[0045] Figure 2 A method flow chart of an embodiment of a method for accurately producing electrolytic copper foil provided by the present invention;
[0046] Figure 3The present invention provides a method flow chart of another embodiment of the method for accurately producing electrolytic copper foil. DETAILED DESCRIPTION
[0047] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0048] In the description of the present application, “plurality” means two or more than two, unless otherwise clearly and specifically defined.
[0049] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0050] The present invention achieves the purpose of precise control by adjusting a parameter such as the electrolytic current intensity during the production process of the electrolytic copper foil.
[0051] The present invention provides an electrolytic copper foil precision production system and an electrolytic copper foil precision production method, which are respectively described below.
[0052] Combination Figure 1 As shown, a specific embodiment of the present invention discloses a precise production system for electrolytic copper foil, including a production execution mechanism 110 and a production control module 120, wherein the production execution mechanism is used to electrolyze to obtain copper foil, the production execution mechanism 110 is electrically connected to the production control module 120, and the production control module includes an efficiency value determination module 121, an initial parameter calculation module 122, a production start module 123 and a production adjustment module 124 which are electrically connected in sequence, wherein:
[0053] The efficiency value determination module 121 is used to obtain a target current efficiency value;
[0054] The initial parameter calculation module 122 is used to obtain the target production specifications, and obtain the initial electrolysis time and the initial current intensity according to the target production specifications, based on the preset electrolysis model and the target current efficiency value;
[0055] The production start module 123 is used to send a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity to control the production execution mechanism to start electrolysis;
[0056] The production adjustment module 124 is used to obtain actual production specifications, and obtain a corrected current intensity based on the actual production specifications and the target production specifications and based on the preset electrolysis model, and send a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0057] The present invention provides an electrolytic copper foil precision production system and an electrolytic copper foil precision production method, wherein the system includes a production execution mechanism and a production control module. During production, a target current efficiency value is first obtained, and then a target production specification is obtained. According to the target production specification, based on a preset electrolysis model and the target current efficiency value, an initial electrolysis time and an initial current intensity are obtained. Then, according to the initial electrolysis time and the initial current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to start electrolysis. Finally, the actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and according to the corrected current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis. Compared with the prior art, the present invention does not use fixed parameters for production, but uses non-fixed current, and adjusts to the corrected current intensity at any time during the production process, so that the production is flexible and more accurate.
[0058] In a preferred embodiment, the production execution mechanism further includes a motor, a reduction transmission mechanism, a cathode roller and an electrolytic cell, the motor is connected to the reduction transmission mechanism, the reduction transmission mechanism is connected to the cathode roller, and the circumference of the cathode roller extends into the electrolytic cell. It is understandable that in the actual production execution mechanism for electrolytic copper foil, the parts other than the above-mentioned parts are all prior art, so this article will not explain them in detail.
[0059] In order to better implement the electrolytic copper foil precision production system in the embodiment of the present invention, based on the previous electrolytic copper foil precision production system embodiment, correspondingly, combined with Figure 2 As shown, the present invention also provides a precise production method of electrolytic copper foil, which is applied to the precise production system of electrolytic copper foil in the previous embodiment, comprising:
[0060] S201, obtaining a target current efficiency value;
[0061] S202, obtaining target production specifications, and obtaining initial electrolysis time and initial current intensity according to the target production specifications, based on a preset electrolysis model and the target current efficiency value;
[0062] S203, sending a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity to control the production execution mechanism to start electrolysis;
[0063] S204, obtaining actual production specifications, and according to the actual production specifications and the target production specifications, based on the preset electrolysis model, obtaining a corrected current intensity, and sending a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0064] In a preferred embodiment, the preset electrolysis model includes:
[0065] M=KITη
[0066] Wherein, M is the production specification, K is the electrochemical equivalent, I is the current intensity, T is the electrolysis time, and η is the current efficiency value. Among them, the production specification M, i.e., the weight of the electrolytic deposition layer, is the specification model of the product, which is measured by the product surface density (gram weight per square centimeter). It is the final product of the production and the final object of quality control. The electrochemical equivalent K refers to the amount of substance precipitated when the same amount of electricity (generally 1C) is passed through different electrolytes. For example, 1g of any substance is equivalent to the amount of electricity passed through 95600C or 26.8A. In this embodiment, the electrochemical equivalent is 1.186g / Ah, which can also be determined according to the specific circumstances in practice. The current intensity I is measured in amperes (A). It is a production condition that can be adjusted and controlled in production, not the final control object. The electrolysis time T is the residence time of the continuously running electrode (cathode roller) in the electrolytic cell. In this embodiment, it can be controlled by the linear speed of the cathode roller. The linear speed of the cathode roller is transmitted through the reduction mechanism using the rotation speed of the motor. Controlling the motor speed is to control the cathode roller linear speed, and indirectly control the electrolysis time. The current efficiency η is a percentage, which changes in real time with the operation of the equipment. It is the main source of interference and should not be replaced by a fixed value at will. It should be accurately calculated and controlled.
[0067] The specific derivation process of the above preset electrolysis model is as follows:
[0068] Faraday's first law of electrolysis: The weight of the substance deposited on the electrode is proportional to the current intensity and the time it passes through, that is, it is proportional to the amount of electricity passing through.
[0069] m=Kit=kQ
[0070] In the formula: m is the amount of substance precipitated (or dissolved) on the electrode / g; I is the current intensity passing through / A; t is the time passing through / h; Q is the amount of electricity passing through / (Ah); and m is the proportional constant.
[0071] Faraday's second law of electrolysis: When the same amount of electricity passes through different electrolytes, the weight of the substance precipitated in multiple solutions is proportional to its chemical equivalent, and 1g of any substance must pass 96500C or 26.8Ah of electricity to precipitate.
[0072]
[0073] In the formula: m is the amount of substance deposited (or dissolved) on the electrode / g; Q is the amount of electricity passed / (Ah); n is the gram equivalent of the substance; F is the amount of electricity required to deposit (or dissolve) 1g of the substance on the electrode during electrolysis.
[0074] The above two formulas can be used to obtain the electrochemical equivalent K:
[0075]
[0076] The above formula indicates that the electrochemical equivalent of each substance is proportional to its atomic weight and inversely proportional to its valence. For variable valence elements, different valence states have different equivalent values, so its electrochemical equivalent is also different. In this embodiment, copper is monovalent.
[0077] Cu + +e=Cu
[0078] Therefore, the electrochemical equivalent of monovalent copper is 63.55 / 2 / 26.8=1.186g / Ah
[0079] Due to the presence of side reactions:
[0080] Zn 2+ +2e→Zn
[0081] 2H + +2e→H 2 ↑
[0082] Thus, there is an efficiency problem with the amount of electricity passed into the electrolytic cell. The actual mass of the precipitated substance is always different from the theoretically calculated weight. The ratio of the actual precipitated weight to the theoretically calculated weight is expressed as a percentage, which is called the current efficiency and is usually represented by "η".
[0083]
[0084] Where m is the actual weight of the precipitated substance / g; I is the current / A; t is the time / h; k is the electrochemical equivalent / [g×(A×h) -1 】.
[0085] Based on the above series of formulas, the preset electrolysis model in this application can be obtained.
[0086] It is understandable that in practice, other models may be selected as the preset electrolysis model according to specific circumstances.
[0087] In a preferred embodiment, the above step S201, obtaining the target current efficiency value, specifically includes:
[0088] Sending a signal to the production execution mechanism to conduct trial production, and obtaining trial production product parameters and actual mechanism state parameters of the production execution mechanism;
[0089] According to the actual mechanism state parameters, an initial current efficiency value is obtained;
[0090] The initial current efficiency value is corrected according to the trial production product parameters to obtain the target current efficiency value.
[0091] In the existing production process, fixed current efficiency values are used for calculation and production guidance. In actual work, the current efficiency is not a fixed value due to the influence of factors such as temperature, pressure, electrolyte concentration, chemical composition (such as chloride ion content, acid content, etc.), electrode and inter-electrode distance, and material and shape of the electrolytic cell. The current efficiency of the same production equipment under different working conditions and at different time periods is also not a fixed value. Using a fixed current efficiency value will cause errors.
[0092] Therefore, in this embodiment, a trial production is carried out before formal production to conduct product inspection. The inspection results (i.e., the trial production product parameters) are combined with the current intensity and cathode roller speed (i.e., the actual mechanism state parameters) during the trial production to obtain the correct current efficiency value (i.e., the initial current efficiency value). Product inspection is carried out at the beginning and end of each batch, and the current efficiency value is corrected (i.e., the target current efficiency value is obtained) to form a closed-loop quality control mode. The above process can be repeated to obtain accurate current efficiency values of different production equipment and different working conditions, eliminating product errors caused by inaccurate current efficiency values.
[0093] Further, in a preferred embodiment, step S204, obtaining the actual production specifications, and obtaining the corrected current intensity based on the preset electrolysis model according to the actual production specifications and the target production specifications, and sending a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis, specifically includes:
[0094] Obtaining a first production deviation value according to the actual production specification and the target production specification;
[0095] According to the first production deviation value and based on the preset electrolysis model, the initial current intensity is corrected to obtain the corrected current intensity;
[0096] A signal is sent to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
[0097] By adjusting the current intensity through the above process, precise control of the production process can be achieved, and the specific principle will be explained in detail later.
[0098] Further, combined with Figure 3 As shown, in a preferred embodiment, before step S204, the method further includes:
[0099] S205, obtaining actual production specifications, and obtaining a corrected electrolysis time according to the actual production specifications and the target production specifications based on the preset electrolysis model, and sending a signal to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
[0100] Although adjusting the electrolysis time can also control the final specifications, its accuracy is far less than adjusting the current intensity. In this embodiment, the electrolysis time is adjusted first, and then the current intensity is adjusted, so as to achieve the effect of coarse adjustment first and then fine adjustment.
[0101] Specifically, in a preferred embodiment, the above-mentioned obtaining the actual production specifications, and obtaining the corrected electrolysis time based on the preset electrolysis model according to the actual production specifications and the target production specifications, and sending a signal to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis, including:
[0102] Obtaining a second production deviation value according to the actual production specification and the target production specification;
[0103] According to the second production deviation value and based on the preset electrolysis model, the initial electrolysis time is corrected to obtain the corrected electrolysis time;
[0104] A signal is sent to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
[0105] There are many specific means for adjusting the electrolysis time, which need to be determined according to the structure of the actual production execution mechanism. Therefore, in combination with the specific structure of the production execution mechanism in the above embodiment, in a preferred embodiment, the above steps send a signal to the production execution mechanism according to the modified electrolysis time to control the production execution mechanism to continue electrolysis, specifically including:
[0106] Obtaining cathode roller specification parameters of the cathode roller;
[0107] According to the cathode roller specification parameters and the corrected electrolysis time, a target cathode roller rotation speed is obtained;
[0108] According to the target cathode roller rotation speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
[0109] Further, in a preferred embodiment, in the above process, according to the target cathode roller speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis, specifically including:
[0110] Obtaining motor specification parameters of the motor and transmission specification parameters of the reduction transmission mechanism;
[0111] Obtaining a target motor speed according to the motor specification parameters, the transmission specification parameters and the target cathode roller speed;
[0112] According to the target motor speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
[0113] The present invention also provides a more detailed embodiment to more clearly illustrate the above steps S204 and S205:
[0114] In the production process of this embodiment, the electrolysis time is the residence time of the continuously running electrode (cathode roller) in the electrolytic cell, and is controlled by the linear speed of the cathode roller. The linear speed is calculated by the motor speed, the reduction ratio of the reduction mechanism, the cathode roller diameter and the pi. Since pi is an irrational number, the calculated linear speed is an approximate value. If this approximate value is directly used for control, product errors will be caused.
[0115] Therefore, in this embodiment, the motor speed is directly controlled, the linear speed of the cathode roller is indirectly controlled, and finally the electrolysis time is controlled. The following results can be obtained through experiments:
[0116] In the device of this embodiment, the cathode roller specification parameters include: cathode roller diameter 2.016 meters, cathode roller width 1.39 meters. The transmission specification parameters include: reduction ratio of the reduction mechanism 1045.3. The motor specification parameters include the upper and lower limits of the motor speed, etc. The electrochemical equivalent is 1.186, and the current efficiency is 97%.
[0117] 1) To produce products with a gram weight of 855, the production current is 34000A and the required line speed is approximately equal to 0.548 meters per minute.
[0118] Using different line speeds around the value range of 0.548, the weight of the products produced is as follows:
[0119] Table 1 Comparison of production results based on different line speeds
[0120] Production current (A) Line speed (m / min) <![CDATA[Grammage (g / m 2 )]]> 34000 0.54 868.5 34000 0.55 852.7 34000 0.56 837.5
[0121] 2) To produce a product with a gram weight of 855, the production current is 34000A and the required motor speed is about 90.53RPM.
[0122] When different motor speeds are used around the value range of 90.53, the weight of the products produced is as follows:
[0123] Table 2 Comparison of production results based on different motor speeds
[0124] Production current (A) Motor speed (RPM) <![CDATA[Grammage (g / m 2 )]]> 34000 90 860.1 34000 91 850.1 34000 92 841.4
[0125] Combining Table 1 and Table 2, it can be seen that when producing products with a gram weight of 855 and a production current of 34000A, the gram weight of the product changes by 15.23 grams for every 0.01m / min adjustment of the line speed (this resolution is the minimum unit that can be controlled in actual production). When the motor speed is adjusted by 1rmp (this resolution is the minimum unit that can be controlled in actual production), the gram weight of the product changes by 9.25 grams. When producing products of the same specifications, different control concepts and methods will result in completely different control effects when controlling different process parameters. Converting the control of line speed into the control of motor speed can improve the control accuracy and eliminate the errors caused by the participation of irrational numbers in calculations.
[0126] Furthermore, in the existing production process, a fixed current intensity is used and the electrolysis time is adjusted for production. It can be seen from the above results that there are errors in the product. Therefore, the present invention does not use a fixed current for production. The following results can be obtained through experiments:
[0127] Based on the same equipment, the cathode roller diameter is 2.016 meters, the cathode roller width is 1.39 meters, the reduction ratio of the reduction mechanism is 1045.3, the electrochemical equivalent is 1.186, and the current efficiency is 97%.
[0128] To produce products with a gram weight of 855, the motor speed is 91RPM, and the required current is 34175.63A. Different current intensities are used near the value range of 34175.63. The gram weights of the products produced are as follows:
[0129] Table 3 Comparison of production results based on different current intensities
[0130] Motor speed (RPM) Current intensity (A) <![CDATA[Grammage (g / m 2 )]]> 91 34175 854.98413 91 34176 855.00915 91 34177 855.03417
[0131] It can be seen from Table 3 that when the current intensity is adjusted by 1A (this resolution is the minimum unit that can be controlled in actual production), the weight of the product changes by 0.025 grams. Obviously, adjusting the current intensity is more accurate than controlling the electrolysis time. It can improve the control accuracy by 4 orders of magnitude and effectively eliminate product errors.
[0132] In the existing production process, the production specifications are first determined, and then the production is carried out with a fixed current intensity. As mentioned above, once the product specifications and current intensity are fixed, the electrolysis time will also be fixed, and the production speed will also be fixed. There is no flexibility in production, and the production speed cannot be adjusted in time according to production needs, and the error is very large.
[0133] Therefore, the present invention selects production specifications, does not use fixed current for production, adopts flexible production speed, and adjusts current intensity in real time. Such a method can adjust the production speed in real time during production, the production has flexibility, and the accuracy of adjustment during the production process is guaranteed by adjusting the current intensity. Specifically, the core of the present invention to improve accuracy is mainly reflected in the following three aspects:
[0134] 1. Change the control line speed to direct control of motor speed.
[0135] 2. Under the condition of fixed current, the original production method of adjusting the line speed is changed to calculating and selecting the appropriate motor speed and flexibly adjusting the current intensity.
[0136] 3. Fixed current efficiency is changed to accurate calculation of current efficiency and real-time closed-loop adjustment.
[0137] The present invention provides an electrolytic copper foil precision production system and an electrolytic copper foil precision production method, wherein the system includes a production execution mechanism and a production control module. During production, a target current efficiency value is first obtained, and then a target production specification is obtained. According to the target production specification, based on a preset electrolysis model and the target current efficiency value, an initial electrolysis time and an initial current intensity are obtained. Then, according to the initial electrolysis time and the initial current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to start electrolysis. Finally, the actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and according to the corrected current intensity, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis. Compared with the prior art, the present invention does not use fixed parameters for production, but uses non-fixed current, and adjusts to the corrected current intensity at any time during the production process, so that the production is flexible and more accurate.
[0138] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A precise production system for electrolytic copper foil, It is characterized in that It includes a production execution mechanism and a production control module, the production execution mechanism is used to electrolyze to obtain copper foil, the production execution mechanism is electrically connected to the production control module, and the production control module includes an efficiency value determination module, an initial parameter calculation module, a production start module and a production adjustment module which are electrically connected in sequence, wherein: The efficiency value determination module is used to obtain a target current efficiency value; The initial parameter calculation module is used to obtain the target production specifications, and according to the target production specifications, based on the preset electrolysis model and the target current efficiency value, obtain the initial electrolysis time and the initial current intensity; The production start module is used to send a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity, so as to control the production execution mechanism to start electrolysis; The production adjustment module is used to obtain the actual production specifications, and obtain the corrected current intensity based on the preset electrolysis model according to the actual production specifications and the target production specifications, and send a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis; The preset electrolysis model includes: M=KITη In the formula M For the production specifications, K is the electrochemical equivalent, I is the current intensity, T is the electrolysis time, η is the current efficiency value.
2. The electrolytic copper foil precision production system according to claim 1, It is characterized in that The production execution mechanism also includes a motor, a reduction transmission mechanism, a cathode roller and an electrolytic cell. The motor is transmission-connected to the reduction transmission mechanism, the reduction transmission mechanism is transmission-connected to the cathode roller, and the circumference of the cathode roller extends into the electrolytic cell.
3. A method for accurately producing electrolytic copper foil, applied to the accurate production system for electrolytic copper foil as claimed in claim 2, It is characterized in that include: Obtaining a target current efficiency value; Obtaining target production specifications, and obtaining an initial electrolysis time and an initial current intensity according to the target production specifications, based on a preset electrolysis model and the target current efficiency value; Sending a signal to the production execution mechanism according to the initial electrolysis time and the initial current intensity to control the production execution mechanism to start electrolysis; The actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected current intensity is obtained, and a signal is sent to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
4. The method for accurately producing electrolytic copper foil according to claim 3, It is characterized in that The obtaining of the actual production specification, and obtaining a corrected current intensity according to the actual production specification and the target production specification based on the preset electrolysis model, and sending a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis, including: Obtaining a first production deviation value according to the actual production specification and the target production specification; According to the first production deviation value and based on the preset electrolysis model, the initial current intensity is corrected to obtain the corrected current intensity; A signal is sent to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis.
5. The method for accurately producing electrolytic copper foil according to claim 3, It is characterized in that Before obtaining the actual production specification, obtaining the corrected current intensity according to the actual production specification and the target production specification based on the preset electrolysis model, and sending a signal to the production execution mechanism according to the corrected current intensity to control the production execution mechanism to continue electrolysis, the method further includes: The actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected electrolysis time is obtained, and a signal is sent to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
6. The method for accurately producing electrolytic copper foil according to claim 5, It is characterized in that The actual production specification is obtained, and according to the actual production specification and the target production specification, based on the preset electrolysis model, a corrected electrolysis time is obtained, and according to the corrected electrolysis time, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis, including: Obtaining a second production deviation value according to the actual production specification and the target production specification; According to the second production deviation value and based on the preset electrolysis model, the initial electrolysis time is corrected to obtain the corrected electrolysis time; A signal is sent to the production execution mechanism according to the corrected electrolysis time to control the production execution mechanism to continue electrolysis.
7. The method for accurately producing electrolytic copper foil according to claim 6, It is characterized in that The sending of a signal to the production execution mechanism according to the modified electrolysis time to control the production execution mechanism to continue electrolysis includes: Obtaining cathode roller specification parameters of the cathode roller; According to the cathode roller specification parameters and the corrected electrolysis time, a target cathode roller rotation speed is obtained; According to the target cathode roller rotation speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
8. The method for accurately producing electrolytic copper foil according to claim 7, It is characterized in that The step of sending a signal to the production execution mechanism according to the target cathode roller speed to control the production execution mechanism to continue electrolysis includes: Obtaining motor specification parameters of the motor and transmission specification parameters of the reduction transmission mechanism; Obtaining a target motor speed according to the motor specification parameters, the transmission specification parameters and the target cathode roller speed; According to the target motor speed, a signal is sent to the production execution mechanism to control the production execution mechanism to continue electrolysis.
9. The method for accurately producing electrolytic copper foil according to claim 3, It is characterized in that The obtaining of the target current efficiency value comprises: Sending a signal to the production execution mechanism to conduct trial production, and obtaining trial production product parameters and actual mechanism state parameters of the production execution mechanism; According to the actual mechanism state parameters, an initial current efficiency value is obtained; The initial current efficiency value is corrected according to the trial production product parameters to obtain the target current efficiency value.
Citation Information
Patent Citations
Metal foil and manufacturing method and manufacturing device thereof
CN101660181A
Preparation method of nano Sn / SiC composite plating
CN102051657A
Adaptive control method for increasing thickness precision of finish-rolled band steel by utilizing roll gap
CN102371279A
Electrolytic copper foil, and lithium ion secondary battery using same
CN107075707A
Device and method for real-time calculation and display of weight of copper foil
CN107761137A