By optimizing the chemical composition and process flow, the problems of high cost and equipment investment in the existing technology have been solved, the production of high-strength, low-cost 1860MPa grade prestressed steel wire has been achieved, and prestressed wire rods with high strength and uniform structure have been obtained.
Patent Information
- Application Number
- CN202310256782.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-17
AI Technical Summary
The existing process cost for producing high-strength prestressed steel wires above 1860MPa level is high, requiring new equipment investment and maintenance costs, and the process is long, and the conventional component design is difficult to meet the performance requirements of large size, high strength, high torsion and low relaxation. .
By optimizing the chemical composition design of the prestressed wire rod, C: 0.90-0.95%, Si: 0.60-0.70%, Mn: 0.40-0.50%, Cr: 0.20-0.25%, V: 0.020-0.040% , Al: 0.025-0.040%, Ti: 0.025-0.040%, combined with the processes of KR pretreatment, BOF converter, LF refining, VD vacuum degassing, continuous casting, controlled rolling and controlled cooling, to achieve high strength, toughness and low-cost production .
Achieved high-strength, low-cost prestressed steel wire production, achieved tensile strength between 1300-1450MPa, area shrinkage ≥ 35%, mesh carbon ≤ 1.0 level, no obvious martensite, bainite structure, Soxhlet The body rate reaches more than 90%, reducing equipment investment and maintenance costs.
Smart Images

Figure CN116479324B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel production, and in particular to a large-size prestressed wire rod for producing prestressed steel wires above 1860MPa level and a production process thereof. Background Art
[0002] Steel strands have the characteristics of high tensile strength, low relaxation value, good elongation and fatigue resistance, and are widely used in the construction of roads, bridges, airports, water conservancy dams, etc. As the uses and use environments of prestressed steel wires and steel strands continue to change, the quality requirements for raw material wire rods are also constantly increasing, especially large-size, high-strength, high-torsion, low-relaxation and other special-purpose steel strands are gradually becoming a hot spot in the market.
[0003] Conventional prestressed wire rod composition design and broad process control requirements can meet the general requirements for the organizational performance of prestressed steel wire and steel strand. However, for prestressed wire rods with special purposes such as large specifications, high strength, high torsion, and low relaxation, the use of conventional composition design and controlled rolling and cooling methods often cannot enable the material to obtain the ideal organization and performance, and often leads to problems such as segregation, abnormal organization, uneven organization, poor plasticity, and large strength fluctuations.
[0004] At present, the mainstream process for producing steel strands with tensile strength exceeding 1860Mpa at home and abroad is to adopt high carbon and high silicon chemical composition design. The strengthening and toughening treatment of the wire rod with this composition design adopts the wire rod re-austenization through offline salt bath / lead bath process or online salt bath treatment process. The advantage of this process is that it reduces the amount of alloy elements, and the austenite-pearlite transformation process is an isothermal transformation, which can obtain a wire rod with high sorbitization rate, fine cementite interlamellar spacing, and uniform organization. The disadvantages are long process flow, high energy consumption, high cost, and the need to set up a new set of online or offline salt (lead) bath equipment, which requires large equipment investment. On this basis, some steel companies have developed a high carbon and low silicon + micro-alloy strengthening composition design, two-fire material + EDC water bath treatment online toughening treatment technology to replace the salt bath / lead bath process. This technology also requires new equipment investment and equipment maintenance is difficult.
[0005] The existing Chinese patent publication number CN105671443A discloses a hot-rolled wire rod and production method for 1960MPa-level cable galvanized steel wire. The tensile strength of the steel wire meets ≥1960MPa, and the torsion index is ≥14 times. It can be used to produce 1960MPa-level bridge cable galvanized steel wire. The patent adopts a large square billet two-fire material process, and the process flow is long and the cost is high. The patent publication number CN113897544A discloses a rare earth high-strength and high-toughness prestressed steel strand wire rod and its smelting and rolling production method. It uses alloy elements such as Cr and V to improve the wire strength. The maximum strength can reach 2000Mpa. At the same time, the addition of rare earth La and Ce elements and the high-draw carbon process improve the center segregation of the ingot, but the process requires the addition of rare earth elements, and the process is complicated and the cost is high. The patent with publication number CN109468530A discloses hot-rolled wire rod and production method for galvanized steel wire for large bridge cables above 2000Mpa. The composition design adopts a high-carbon and low-silicon composition system, adds micro-alloying elements, adopts large square billets and two-fire material forming, and online EDC water bath toughening treatment cooling method. This process equipment has high investment and maintenance costs, and the cost of two-fire material forming is high. The patent with publication number CN112267069A discloses wire rod and manufacturing method for 2100Mpa cable steel wire. This patent adopts a high-carbon, high-silicon and low-chromium composition design, and adopts an offline salt bath or lead bath treatment process. The process cost is high, the production efficiency is low, and a salt bath production line is required, and the equipment maintenance cost is high.
[0006] In summary, the existing production cost of high-strength prestressed steel wire above 1860Mpa is relatively high, requires new equipment investment and maintenance costs, and has a long process flow. Summary of the invention
[0007] In view of the defects of the above-mentioned prior art, the present invention provides a large-size prestressed wire rod and a production process thereof for producing prestressed steel wire of a grade above 1860MPa. Without building new salt bath / lead bath equipment, the existing rolling and air cooling equipment of the steel plant is utilized, and the composition of the prestressed wire rod is optimized to produce a wire rod for cables with high strength, toughness and plasticity, simple composition, simplified process, green and low carbon, and high production efficiency.
[0008] In the first aspect, the present invention provides a large-size prestressed wire rod for producing prestressed steel wires of 1860 MPa or above, using the following technical solution:
[0009] A large-size prestressed wire rod for producing prestressed steel wires of a grade above 1860 MPa, wherein the chemical composition of the prestressed wire rod is as follows by weight percentage: C: 0.90-0.95%, Si: 0.60-0.70%, Mn: 0.40-0.50%, Cr: 0.20-0.25%, V: 0.020-0.040%, Al: 0.025-0.040%, Ti: 0.025-0.040%, P≤0.010%, S≤0.0050%, N≤40ppm, TO: 10-30ppm, H≤1ppm, and the rest are Fe and unavoidable residual elements; (Cr+Mn+V*10)≤0.9, (Al+Ti) / N≥1.5.
[0010] By adopting the above technical solution: Compared with the design ideas of ordinary high carbon, high silicon and micro-alloying components, this application further increases the content of C and Si elements, and reduces the content of Mn, Cr and V elements to obtain high-strength prestressed wire rod. Since it is difficult for Mn, Cr and V elements to reduce the segregation of the ingot by high-temperature diffusion, when Mn, Cr and V elements are added excessively, segregation is likely to occur and the hardenability of the organization will increase, resulting in the appearance of abnormal organizations such as martensite and bainite in the organization. Therefore, the content of these three elements must be controlled and the condition of (Cr+Mn+V*10)≤0.9 must be met. When the Mn content exceeds 0.50%, the austenite will coarsen when the wire rod is heated. After the austenite grains are coarsened, the grains of the steel will be coarse after heat treatment, which will reduce the mechanical properties of the steel; Cr is an element that strongly increases the incubation time before the austenite transformation. The increase in incubation time will increase the risk of abnormal martensite organization, so it is strictly controlled below 0.25% in this application.
[0011] The addition of Al and Ti elements in this application can generate Al 2 O 3 , AlN, TiN and other finely dispersed refractory compounds can be used to refine the austenite recrystallized grains. At the same time, it can also inhibit the coarsening of austenite grains during heating and rolling, and combined with a lower finishing temperature, obtain austenite grains before phase transformation of ≤30μm. The refined austenite grains can increase the grain boundary area and reduce the adverse effects of proeutectoid cementite. At the same time, the refined austenite grains will reduce the incubation time, thereby reducing abnormal structures such as martensite.
[0012] In summary, the combined use of the above-mentioned chemical elements in the present application makes the tensile strength of the prestressed wire rod obtained in the present application between 1300-1450MPa, the area reduction ≥35%, the net carbon ≤1.0 level, and no obvious martensite and bainite structure.
[0013] In the second aspect, the present invention provides a production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above, comprising the following steps:
[0014] KR pretreatment, BOF converter, LF refining, VD vacuum degassing, continuous casting, billet heating, controlled rolling and cooling treatment, DP controlled cooling treatment;
[0015] The controlled rolling and controlled cooling treatment includes: the inlet temperature of the finishing mill is 920-960℃, the inlet temperature of the sizing reduction mill is 900-940℃, and the wire laying temperature is 830-860℃;
[0016] During DP controlled cooling treatment: after spinning, the wire rod enters the Stelmor cooling line, the cooling rate before phase change is 15-20℃ / S, the phase change temperature is 560-580℃, the red-returning temperature after phase change is 600-610℃, the cooling rate after phase change and red-returning is 0.5-1℃ / s, and the opening degree of Jialing is controlled at 30%.
[0017] By adopting the above technical scheme, the coordinated use of the finishing mill inlet temperature, sizing inlet temperature, spinning temperature, cooling rate before phase change, phase change temperature, red-returning temperature after phase change, and cooling rate after phase change and red-returning in the controlled rolling and cooling treatment can make the prestressed steel have a troostite rate of more than 90%, and the troostite structure is fine and uniform, without abnormal structure, so that the mechanical properties of the wire rod are stable.
[0018] Preferably, the air cooling parameters in the DP controlled cooling treatment are: fan air volume is turned on at 100% for fans 1-3, 90% for fans 4-8, the remaining fans are turned off, and the insulation cover after fan No. 9 is turned off; the roller speed is set as follows: the first roller speed is 0.90-0.95m / s, the roller speeds of sections 2-4 are increased by 10% in sequence, the roller speeds of sections 5-6 are increased by 5% in sequence, and the speeds of the remaining rollers remain unchanged.
[0019] Preferably, the temperature of the soaking section during the heating of the steel billet is 1180-1220° C., the total heating time is 130-170 min, and the heating time in the soaking section is ≥45 min.
[0020] By adopting the above technical solution, when the temperature of the soaking section is set within the range of 1180-1220°C, the segregation of the ingot can be reduced, the composition can be homogenized, and at the same time, the V and Cr alloys can be completely dissolved.
[0021] Preferably, the BOF converter uses low-phosphorus and high-carbon steel, the converter tapping temperature is ≤1640°C, the converter endpoint C content is 0.15-0.40%, and P is ≤0.010%.
[0022] Preferably, in the LF refining process, low basicity refining slag is used, ferrosilicon alloy is deoxidized, Al particles are added after deoxidation, so that the total Al content in the LF furnace steel composition is controlled at 0.030-0.045%, and the LF refining soft blowing time is greater than 35 minutes.
[0023] Preferably, in the VD vacuum degassing process, the vacuum degree is ≤67 Pa, the vacuum holding time is ≥15 min, and the soft blowing time is ≥15 min.
[0024] Preferably, the continuous casting adopts a crystallizer, end electromagnetic stirring, secondary cooling, and low superheat casting, the superheat is controlled at 15-25°C, the pulling speed is 1.25m / min, the crystallizer water volume is 1100m3 / h, and the secondary cooling water volume is 0.30L / kg.
[0025] Preferably, after the continuous casting process, the continuous casting billet is slowly cooled for 48 hours and then the billet is heated.
[0026] By adopting the above technical solution, the present application adopts a lower spinning temperature to inhibit the precipitation of network cementite, and then enters the Stelmor cooling line, adopts a large air volume fan and a higher roller speed to increase the cooling rate before phase transformation, and then cooperates with fine austenite grains to obtain a fine and uniform troostite structure, so that the troostite rate of the wire rod reaches more than 90%. After the phase transformation, in order to avoid the residual austenite from being overcooled to produce martensite structure, the cooling rate after the phase transformation is minimized by closing the No. 8 rear fan and closing the heat preservation cover, while increasing the temperature of the aggregate coil and reducing the aging period of the prestressed wire rod.
[0027] In addition, in order to control the segregation of the ingot, the present application adopts plasma tundish heating, low superheat, high temperature and long-term heating diffusion, so that the C segregation index of the ingot can be reduced to within 1.08.
[0028] In summary, the present invention has the following beneficial effects:
[0029] Through component design and process design, the present invention enables the prestressed wire rod of the present invention to achieve the performance that previously required double-fired materials or salt baths, lead baths, EDC water baths, etc. to achieve by using single-fired materials and Stelmor air cooling process, thereby greatly reducing production costs and reducing process complexity. At the same time, the matching of component design and process design in the present invention enables the prestressed wire rod obtained by the present invention to obtain fine and uniform troostite clusters, with a troostite rate of more than 90% and no obvious martensite and bainite structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Metallographic structure test diagram of the prestressed wire rod obtained in Example 1. DETAILED DESCRIPTION
[0031] The following is combined with the embodiment and Figure 1 The present invention is described in further detail.
[0032] Example 1
[0033] A production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above, comprising the following steps:
[0034] (1) KR hot metal pretreatment, so that the hot metal composition is P: 0.0062%, S: 0.0017%, Cu: 0.016%, Cr: 0.051%; (2) BOF converter, specifically, a 120-ton converter is charged with 113 tons of hot metal and 8 tons of scrap steel, and then 1050 kg of quartzite is added to the converter. During the blowing process, 3500 kg of lime, 900 kg of dolomite and sintered ore are added. The sintered ore is adjusted according to the charge temperature, so that the converter end point C content is 0.15%, P ≤ 0.010%, and the end point oxygen content is 430 ppm. The end point control adopts high carbon and low temperature steelmaking, and re-blowing is prohibited. The carbon pulling temperature is 1 593℃, the tapping temperature is 1615℃, and the temperature before argon blowing is 1526℃; alloying is carried out during the tapping process of the converter, and the bottom blowing of the ladle is controlled within 350mm. After the alloy is melted, the bottom blowing of the ladle is closed. When the amount of molten steel in the ladle is about 25t, the following alloys and slag are added in sequence: ferrosilicon, carburizer, medium carbon ferromanganese, ferrochrome, ferrovanadium, ferrotitanium, aluminum particles, and top slag, so that the composition of the molten steel reaches C: 0.8559%, Si: 0.5136%, Mn: 0.3886%, P: 0.008%, S: 0.0043%, Al: 0.0186%, Cr: 0.2233%, V: 0.0224%;
[0035] (3) LF refining, in which low basicity refining slag (CaO:SiO) is used in the refining process 2 1-2), the bottom blowing argon flow rate is 250L / min, the soft blowing argon flow rate is 200L / min, the soft blowing time is 40min, the soft blowing intensity is preferably such that the top slag molten steel is not exposed, after temperature measurement and sampling, according to the results, ferrosilicon alloy is added for deoxidation according to the composition of the target prestressed steel, and Al particles are added after deoxidation, so that the total Al content in the LF furnace steel composition is controlled at 0.030%;
[0036] (4) VD vacuum degassing, vacuum degree is 67Pa, vacuum holding time is 15min, soft blowing time is 15min, Ca treatment is not allowed, so as to improve the purity of steel;
[0037] (5) Continuous casting process: plasma tundish heating is adopted. The process starts when the tundish temperature is lower than 1474℃ and stops when it is higher than 1484℃. The superheat is controlled within the range of 15-25℃. The constant casting speed is 1.25m / min and the water volume of the crystallizer is 1100m 3 / h, secondary cooling water volume 0.30L / kg, crystallizer electromagnetic stirring flow rate 450A, frequency 2.4Hz, terminal electromagnetic stirring setting current 450A, frequency 10Hz;
[0038] The ingot is transported to the holding pit and slowly cooled for 48 hours;
[0039] (6) Billet heating: the prestressed billet is added into the heating furnace, enters from the preheating section, passes through the heating section, and is output from the soaking section, wherein the temperature of the preheating section is 550° C., the temperature of the heating section is 1208° C., the temperature of the soaking section is 1180° C., the total heating time is 155 min, the high temperature diffusion heating time is 45 min, and the residual oxygen content is 1.2%;
[0040] (7) controlled rolling and controlled cooling treatment, the steel obtained in step (7) is subjected to 6+8 rough rolling, 4 pre-finishing rolling, 8 finishing rolling, the starting rolling temperature is 1164°C, the finishing mill inlet temperature is 920°C, the sizing inlet temperature is 940°C, and the wire drawing temperature is 830°C; (8) DP controlled cooling treatment, after the wire drawing, the wire rod enters the Stelmor cooling line, wherein the air cooling parameter in the DP controlled cooling treatment is 260,000 m 3 / h centrifugal fans 1-3 are opened 100%, 4-8 are opened 90%, and the other fans are closed. The insulation cover after fan No. 9 is closed, and the roller speed is set to 0.90m / s for the first roller speed, and the roller speeds of sections 2-4 are increased by 10% in sequence, and the roller speeds of sections 5-6 are increased by 5% in sequence. The speeds of the other rollers remain unchanged, so that the cooling rate of the wire rod before phase change is controlled in the range of 15-20℃ / s, the phase change temperature is 565℃, and the red-return temperature after phase change is 600℃. The cooling rate after red-return is controlled in the range of 0.5-1℃ / s, and the opening degree of Jialing is controlled to 30% to ensure uniform cooling rates at the edge and center. The chemical composition of the prestressed wire rod finally obtained is shown in Table 1.
[0041] Example 2
[0042] A production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above, comprising the following steps:
[0043] (1) KR hot metal pretreatment, so that the hot metal composition is P: 0.0034%, S: 0.0028%, Cu: 0.015%, Cr: 0.044%; (2) BOF converter, specifically, a 120-ton converter is charged with 113 tons of hot metal and 8 tons of scrap steel, and then 1050 kg of quartzite is added to the converter. During the blowing process, 3500 kg of lime, 900 kg of dolomite and sintered ore are added. The sintered ore is adjusted according to the charge temperature, so that the converter end point C content is 0.20%, P ≤ 0.010%, and the end point oxygen content is 450 ppm. The end point control adopts high carbon and low temperature steelmaking, and re-blowing is prohibited. The carbon pulling temperature is 1596℃, tapping temperature is 1613℃, and pre-argon temperature is 1520℃; alloying is carried out during the tapping process of the converter, and the bottom blowing of the ladle is controlled within 350mm. After the alloy is melted, the bottom blowing of the ladle is closed. When the amount of molten steel in the ladle is about 25t, the following alloys and slag are added in sequence: ferrosilicon, carburizer, medium carbon ferromanganese, ferrochrome, ferrovanadium, ferrotitanium, aluminum particles, and top slag, so that the composition of the molten steel reaches C: 0.8617%, Si: 0.5286%, Mn: 0.3535%, P: 0.01%, S: 0.0045%, Al: 0.0189%, Cr: 0.2346%, V: 0.0236%;
[0044] (3) LF refining, in which low basicity refining slag (CaO:SiO) is used in the refining process 2 1-2), the bottom blowing argon flow rate is 250L / min, the soft blowing argon flow rate is 200L / min, the soft blowing time is 40min, the soft blowing intensity is preferably such that the top slag molten steel is not exposed, after temperature measurement and sampling, according to the results, ferrosilicon alloy is added for deoxidation according to the composition of the target prestressed steel, and Al particles are added after deoxidation, so that the total Al content in the LF furnace steel composition is controlled at 0.038%;
[0045] (4) VD vacuum degassing, vacuum degree is 60Pa, vacuum holding time is 18min, soft blowing time is 20min, Ca treatment is not allowed, so as to improve the purity of steel;
[0046] (5) Continuous casting process: plasma tundish heating is adopted. The process starts when the tundish temperature is lower than 1474℃ and stops when it is higher than 1484℃. The superheat is controlled within the range of 15-25℃. The constant casting speed is 1.25m / min and the water volume of the crystallizer is 1100m 3 / h, secondary cooling water volume 0.30L / kg, crystallizer electromagnetic stirring flow rate 450A, frequency 2.4Hz, terminal electromagnetic stirring setting current 450A, frequency 10Hz;
[0047] The ingot is transported to the holding pit and slowly cooled for 48 hours;
[0048] (6) Billet heating: the prestressed billet is added into the heating furnace, enters from the preheating section, passes through the heating section, and is output from the soaking section. The temperature of the preheating section is 551°C, the temperature of the heating section is 1204°C, the temperature of the soaking section is 1202°C, the total heating time is 152 minutes, the heating time of the soaking section is 50 minutes, and the residual oxygen content is 1.4%;
[0049] (7) controlled rolling and controlled cooling treatment, the steel obtained in step (7) is subjected to 6+8 rough rolling, 4 pre-finishing rolling, 8 finishing rolling, the starting rolling temperature is 1156°C, the finishing mill inlet temperature is 950°C, the sizing inlet temperature is 930°C, and the wire drawing temperature is 844°C; (8) DP controlled cooling treatment, after the wire drawing, the wire rod enters the Stelmor cooling line, wherein the air cooling parameter in the DP controlled cooling treatment is 260,000 m 3 / h centrifugal fans No. 1-3 are opened 100%, No. 4-8 are opened 90%, and the other fans are closed. The insulation cover after No. 9 fan is closed, and the roller speed is set to 0.90m / s for the first roller speed, and the roller speeds of sections 2-4 are increased by 10% in sequence, and the roller speeds of sections 5-6 are increased by 5% in sequence. The speeds of the other rollers remain unchanged, so that the cooling rate of the wire rod before phase change is controlled in the range of 15-20℃ / s, the phase change temperature is 560℃, and the red-returning temperature after phase change is 610℃. The cooling rate after red-returning is controlled in the range of 0.5-1℃ / s, and the opening degree of Jialing is controlled to 30% to ensure uniform cooling rates at the edge and center. The chemical composition of the prestressed wire rod finally obtained is shown in Table 1.
[0050] Example 3
[0051] A production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above, comprising the following steps:
[0052] (1) KR hot metal pretreatment, so that the hot metal composition is P: 0.0066%, S: 0.0023%, Cu: 0.016%, Cr: 0.041%; (2) BOF converter, specifically, a 120-ton converter is charged with 113 tons of hot metal and 8 tons of scrap steel, and then 1050 kg of quartzite is added to the converter. During the blowing process, 3500 kg of lime, 900 kg of dolomite and sintered ore are added. The sintered ore is adjusted according to the charge temperature, so that the converter end point C content is 0.40%, P ≤ 0.010%, and the end point oxygen content is 470 ppm. The end point control adopts high carbon and low temperature steelmaking, and re-blowing is prohibited. The carbon pulling temperature is 1 585℃, tapping temperature is 1616℃, and pre-argon temperature is 1525℃; alloying is carried out during the tapping process of the converter, and the bottom blowing of the ladle is controlled within 350mm. After the alloy is melted, the bottom blowing of the ladle is closed. When the amount of molten steel in the ladle is about 25t, the following alloys and slag are added in sequence: ferrosilicon, carburizer, medium carbon ferromanganese, ferrochrome, ferrovanadium, ferrotitanium, aluminum particles, and top slag, so that the composition of the molten steel reaches C: 0.8529%, Si: 0.5627%, Mn: 0.3506%, P: 0.0103%, S: 0.0031%, Al: 0.0194%, Cr: 0.2391%, and V: 0.0251%;
[0053] (3) LF refining, in which low basicity refining slag (CaO:SiO) is used in the refining process 2 1-2), the bottom blowing argon flow rate is 250L / min, the soft blowing argon flow rate is 200L / min, the soft blowing time is 40min, the soft blowing intensity is preferably such that the top slag molten steel is not exposed, after temperature measurement and sampling, according to the results, ferrosilicon alloy is added for deoxidation according to the composition of the target prestressed steel, and Al particles are added after deoxidation, so that the total Al content in the LF furnace steel composition is controlled at 0.030-0.045%;
[0054] (4) VD vacuum degassing, vacuum degree is 62Pa, vacuum holding time is 20min, soft blowing time is 20min, Ca treatment is not allowed, so as to improve the purity of steel;
[0055] (5) Continuous casting process: plasma tundish heating is adopted. The process starts when the tundish temperature is lower than 1474℃ and stops when it is higher than 1484℃. The superheat is controlled within the range of 15-25℃. The constant casting speed is 1.25m / min and the water volume of the crystallizer is 1100m 3 / h, secondary cooling water volume 0.30L / kg, crystallizer electromagnetic stirring flow rate 450A, frequency 2.4Hz, terminal electromagnetic stirring setting current 450A, frequency 10Hz;
[0056] The ingot is transported to the holding pit and slowly cooled for 48 hours;
[0057] (6) Billet heating: the prestressed billet is added into the heating furnace, enters from the preheating section, passes through the heating section, and is output from the soaking section. The temperature of the preheating section is 551°C, the temperature of the heating section is 1204°C, the temperature of the soaking section is 1220°C, the total heating time is 170 min, the heating time of the soaking section is 60 min, and the residual oxygen content is 1.4%;
[0058] (7) controlled rolling and controlled cooling treatment, the steel obtained in step (7) is subjected to 6+8 rough rolling, 4 pre-finishing rolling, 8 finishing rolling, the starting rolling temperature is 1154°C, the finishing mill inlet temperature is 960°C, the sizing inlet temperature is 940°C, and the wire drawing temperature is 860°C; (8) DP controlled cooling treatment, after the wire drawing, the wire rod enters the Stelmor cooling line, wherein the air cooling parameter in the DP controlled cooling treatment is 260,000 m 3 / h centrifugal fans 1-3 are opened 100%, 4-8 are opened 90%, and the other fans are closed. The insulation cover after fan No. 9 is closed, and the roller speed is set to 0.9m / s for the first roller speed, and the roller speeds of sections 2-4 are increased by 10% in sequence, and the roller speeds of sections 5-6 are increased by 5% in sequence. The speeds of the other rollers remain unchanged, so that the cooling rate of the wire rod before phase change is controlled in the range of 15-20℃ / s, the phase change temperature is 580℃, and the red-returning temperature after phase change is 610℃. The cooling rate after red-returning is controlled in the range of 0.5-1℃ / s, and the opening degree of Jialing is controlled to 30% to ensure uniform cooling rates at the edge and center. The chemical composition of the prestressed wire rod finally obtained is shown in Table 1.
[0059] Table 1 Chemical composition of prestressed steel (wt%)
[0060]
[0061] Comparative Example 1
[0062] The difference from Example 1 is that the content of Cr element in the chemical composition of the prestressed steel is 0.50%, and the contents of other chemical components are the same as those in Example 1.
[0063] Comparative Example 2
[0064] The difference from Example 1 is that there is no V element in the chemical composition of the prestressed steel and the content of Cr element is 0.50%, and the contents of other chemical components are the same as in Example 1.
[0065] Comparative Example 3
[0066] The difference from Example 1 is that the content of Mn element in the chemical composition of the prestressed steel is 0.60%, and the contents of other chemical components are the same as those in Example 1.
[0067] Comparative Example 4
[0068] The difference from Example 1 is that the chemical composition of the prestressed steel does not contain Ti and V elements, and the contents of other chemical components are the same as those in Example 1.
[0069] Comparative Example 5
[0070] The difference from Example 1 is that in step (7) the controlled rolling and controlled cooling treatment, the finishing mill inlet temperature is 970°C and the sizing inlet temperature is 950°C, and the remaining steps are the same as in Example 1.
[0071] Comparative Example 6
[0072] The difference from Example 1 is that in step (7) the controlled rolling and controlled cooling treatment, the inlet temperature of the finishing mill is 910°C and the inlet temperature of the sizing reduction mill is 890°C, and the remaining steps are the same as in Example 1.
[0073] Comparative Example 7
[0074] The difference from Example 1 is that in step (7) the controlled-spinning and controlled-cooling treatment, the spinning temperature is 820°C, and the remaining steps are the same as in Example 1.
[0075] Comparative Example 8
[0076] The difference from Example 1 is that in step (7) the controlled-spinning and controlled-cooling treatment, the spinning temperature is 870°C, and the remaining steps are the same as in Example 1.
[0077] Comparative Example 9
[0078] The difference from Example 1 is that the DP process in Example B of the current Chinese patent CN114657471A is adopted in step (8) DP controlled cooling treatment, that is, the air cooling parameters are 100% for 1-6 fans, 95-100% for 7-12 fans, 80-100% for 13-16 fans, 1-10 fans with nozzle water flow in front of the damper, 0.95-1.50 MPa of compressed air, cooling speed of different fans before phase change is 15.1-17.7°C / s, and temperature before phase change (before returning to temperature) is 584-600°C.
[0079] Performance Testing
[0080] The prestressed steel obtained in the embodiment and the comparative example was rolled into a wire rod with a specification of φ14mm. After an aging period of 15 days, 20 wire rod samples were taken for performance testing. The test results are shown in Table 2, where the tensile strength and elongation tests were carried out in accordance with the relevant provisions of GB / T228.1-2010. The test is based on GB / T13298-2015 "Methods for the inspection of metal microstructures"; the martensite rating is based on YB / T4411-2014 "Method for the evaluation of central martensite in high carbon steel wire rods". The depth of the decarburized layer is carried out in accordance with the provisions of GB / T224-2019. The detection of non-metallic inclusions in steel is based on the relevant provisions of GB / T10561-2005 "Standard rating chart microscopic inspection method for the determination of non-metallic inclusion content in steel". Class A is sulfide inclusions; Class B is alumina inclusions; Class C is silicate inclusions; Class D is spherical oxide inclusions.
[0081] Table 2 Prestressed wire rod test results
[0082]
[0083]
[0084] Table 2 Prestressed wire rod inclusion test results, unit: grade
[0085]
[0086]
[0087] The prestressed wire rods obtained in the examples and comparative examples were made into 5.33 mm 1860 MPa grade galvanized steel wires, and the test results are shown in Table 3.
[0088] Table 3 5.33mm 1860Mpa galvanized steel wire
[0089]
[0090] The prestressed wire rods obtained in the examples and comparative examples were made into 7 mm 1860 MPa grade galvanized steel wires, and the test results are shown in Table 4.
[0091] Table 4 7mm 1860Mpa galvanized steel wire
[0092]
[0093] Combining Table 2, Table 3 and Table 4, we can see that:
[0094] The various properties of the prestressed wire rod obtained in the embodiments of the present application are better than those of the prestressed wire rod obtained in the comparative examples, indicating that the combination of the components and processes in the present application can stably produce 1860Mpa galvanized steel wire, and the torsion times of the finally obtained 5.33mm 1860Mpa galvanized steel wire and 7mm 1860Mpa galvanized steel wire are both greater than 14, and the strength is stable and the structure is uniform.
[0095] Compared with Example 1, when the contents of Cr, Mn, V, and Ti are changed so as to be out of the range defined in the present application, the martensitic structure of the prestressed wire rods obtained in Comparative Examples 1-4 increases, and the content of inclusions in the wire rods also increases, which ultimately leads to a decrease in the tensile strength and torsion times of the galvanized steel wire, so that the performance of the steel wire does not meet the requirements. It can be seen that effective control of the contents of Cr, Mn, V, and Ti can effectively reduce the probability of abnormal tissue appearing in the steel tissue.
[0096] Compared with Example 1, in Comparative Examples 5-9, when the finishing mill inlet temperature, the sizing inlet temperature or the spinning temperature or the parameters in the controlled cooling treatment are not within the range specified in this application, the performance of the prestressed wire rod finally obtained is relatively poor, resulting in the steel wire being unable to meet the 1860Mpa grade use requirements.
[0097] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above, characterized in that: The steps include: KR pretreatment, BOF converter, LF refining, VD vacuum degassing, continuous casting, billet heating, controlled rolling and controlled cooling treatment, DP controlled cooling treatment; Among them, the controlled rolling and controlled cooling treatment: the inlet temperature of the finishing mill is 920-960℃, the inlet temperature of the sizing reduction mill is 900-940℃, and the spinning temperature is 830-860℃; During DP controlled cooling treatment: after spinning, the wire rod enters the Stelmor cooling line, the cooling rate before phase change is 15-20℃ / s, the phase change temperature is 560-580℃, the red-returning temperature after phase change is 600-610℃, the cooling rate after phase change is 0.5-1℃ / s, and the Jialing opening degree is controlled to be 30%; The chemical composition of the prestressed wire rod is calculated by weight percentage as follows: C: 0.90-0.95%, Si: 0.60-0.70%, Mn: 0.40-0.50%, Cr: 0.20-0.25%, V: 0.020-0.040%, Al: 0.025-0.040%, Ti: 0.025-0.040%, P≤0.010%, S≤0.0050%, N≤40ppm, TO: 10-30ppm, H≤1ppm, and the rest are Fe and unavoidable residual elements, and (Cr+Mn+V*10)≤0.9, (Al+Ti) / N≥1.
5.
2. A production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: The air cooling parameters in the DP controlled cooling treatment are: the air volume of fans No. 1-3 is 100%, the air volume of fans No. 4-8 is 90%, the other fans are all closed, and the insulation cover after fan No. 9 is closed; the roller speed is set as: the first roller speed is 0.90-0.95m / s, the roller speeds of sections 2-4 are increased by 10% in sequence, the roller speeds of sections 5-6 are increased by 5% in sequence, and the speeds of the other rollers remain unchanged.
3. The production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: The temperature of the soaking section during the heating of the steel billet is 1180-1220° C., the total heating time is 130-170 min, and the heating time of the soaking section is ≥45 min.
4. The production process for producing large-size prestressed wire rods of prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: The BOF converter uses low-phosphorus and high-carbon steel, the converter tapping temperature is ≤1640°C, the converter end point C content is 0.15-0.40%, and P is ≤0.010%.
5. The production process for producing large-size prestressed wire rods for prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: In the LF refining process, low basicity refining slag is used, ferrosilicon alloy is deoxidized, Al particles are added after deoxidation, so that the total Al content in the LF furnace steel composition is controlled at 0.030-0.045%, and the LF refining soft blowing time is greater than 35 minutes.
6. The production process for producing large-size prestressed wire rods for prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: In the VD vacuum degassing process, the vacuum degree is ≤67Pa, the vacuum holding time is ≥15min, and the soft blowing time is ≥15min.
7. The production process for producing large-size prestressed wire rods for prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: The continuous casting adopts a crystallizer, end electromagnetic stirring, secondary cooling, weak cooling, and low superheat pouring. The superheat is controlled at 15-25°C, the casting speed is 1.25m / min, and the crystallizer water volume is 1100m 3 / h, secondary cooling water volume 0.30L / kg.
8. The production process for producing large-size prestressed wire rods for prestressed steel wires of 1860 MPa or above according to claim 1, characterized in that: After the continuous casting process, the continuous casting billet is slowly cooled for 48 hours and then the billet is heated.
9. A prestressed wire rod obtained by the production process for producing large-size prestressed wire rods of prestressed steel wires above 1860 MPa grade as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Hot-rolled wire rod for 1,960MPa-level cable rope galvanized steel wire and production method
CN105671443A
Hot-rolled steel wire rod for large bridge cable rope zinc-plated steel wire over 2000 MPa level and production method
CN109468530A
Steel wire rod for 2,100 MPa-grade galvanized steel wire and manufacturing method thereof
CN112267069A
Wire rod for rare earth high-strength and high-toughness prestressed steel strand and smelting and rolling production method of wire rod
CN113897544A
Production method of low-carbon and energy-saving steel wire rod for bridge cable with pressure larger than or equal to 2060 Mpa
CN114657471A