Porous substrates for diaphragms and diaphragms for electrochemical devices containing them
By designing a porous substrate with uniform porosity and pore size, the deformation problem of lithium-ion battery separators under high-pressure lamination conditions was solved, achieving high dielectric breakdown voltage and low deformation rate, thus improving battery performance and safety.
Patent Information
- Application Number
- CN202280007242.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-07
- Filing Date
- 2022-05-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-05-06
AI Technical Summary
Existing lithium-ion battery separators are prone to deformation under high-pressure lamination conditions, which leads to reduced battery performance and decreased dielectric breakdown voltage. There is a need to develop a porous substrate for separators with low thickness deformation rate and high dielectric breakdown voltage.
It uses a porous substrate with a porosity in the range of 30% to 60% by volume, a Gaussian full width at half maximum (FWHM) value of less than 4.0 nm for the pore size distribution, uniform pore size, contains polyethylene and/or polypropylene, has a thickness in the range of 5 to 20 μm, and can be equipped with a heat-resistant layer to improve stability.
Under high-pressure lamination conditions, the membrane thickness of the porous substrate changes little and the dielectric breakdown voltage is high, ensuring the stability and safety of the battery.
Smart Images

Figure CN116491020B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2021-0059551, filed on May 7, 2021. This disclosure relates to a separator for an electrochemical device, wherein the electrochemical device can be a primary battery or a secondary battery, and the secondary battery can include a lithium-ion secondary battery. Background Technology
[0002] Polyolefin microporous membranes are widely used in applications such as battery separators for lithium-ion batteries, separators for electrolytic capacitors, breathable and waterproof clothing, and various filter membranes. When using such polyolefin microporous membranes as battery separators, their performance is closely related to battery characteristics, productivity, and safety. Therefore, lithium-ion battery separators, in particular, need not only excellent mechanical properties and air permeability, but also pore-closing function (pore-closing characteristic) and heat shrinkage resistance. The pore-closing function refers to the ability of the separator's pores to close due to abnormal heating, thereby stopping the battery reaction and preventing battery overheating, fire, and rupture accidents caused by short circuits or overcharging from external circuits. Heat shrinkage resistance refers to the ability of the separator to maintain its shape even at high temperatures to prevent dangerous situations where the positive and negative electrode materials react directly.
[0003] Typically, microporous membranes made solely of polyethylene have low melting temperatures, while microporous membranes made solely of polypropylene have high pore-closing temperatures. Therefore, battery separators composed of microporous membranes made primarily of polyethylene and polypropylene have been proposed.
[0004] For example, Japanese Patent No. 3235669 discloses a battery separator with excellent heat shrinkage resistance and closed-cell properties. The separator comprises: at least one first layer formed of a polymer selected from low-density polyethylene, ethylene-butene copolymer and ethylene-hexene copolymer; and at least one second layer formed of a polymer selected from high-density polyethylene, ultra-high molecular weight polyethylene and polypropylene.
[0005] For example, Japanese Patent No. 3422496 discloses a battery separator with excellent closed-cell properties. The separator comprises: at least one first layer formed of a polymer selected from ethylene-butene copolymer, ethylene-hexene copolymer, ethylene-methacrylate copolymer and polyethylene; and at least one second layer formed of a polymer selected from polyethylene and polypropylene.
[0006] Japanese Patent No. 2883726 discloses a battery separator with excellent closed-cell and melting characteristics. Polypropylene with a melting point of 150°C or higher and polyethylene with a melting point of 100°C to 140°C are simultaneously extruded, and the resulting laminate is unidirectionally stretched at a temperature of -20°C [the melting point of polyethylene (Tm0) - 30°C], and further stretched in the same direction at a temperature of (Tm0 - 30)°C to (Tm0 - 2)°C to form a porous structure.
[0007] Japanese Patent Application Publication No. 11-329390 discloses a battery separator with excellent closed-cell characteristics and strength. This battery separator comprises two polypropylene microporous reinforcing layers and a polyethylene barrier layer containing filler inserted therebetween, wherein the polyethylene barrier layer is composed of a microporous membrane manufactured by particle stretching.
[0008] Batteries are manufactured by bonding such a separator to electrodes, and this bonding is performed through a lamination process, in which electrodes and separators are stacked, and then heat and pressure are applied to the laminate. The higher the heat and pressure applied during the lamination process, the stronger the adhesion to the electrodes. Recently, to improve productivity, process speeds have been increased, resulting in shorter times for applying heat to the separator. Therefore, pressure has been increased to obtain satisfactory adhesion strength. This leads to problems with separator deformation due to high pressure. In particular, when using porous substrates for separators that are susceptible to heat and pressure, significant thickness reduction and pore damage occur. Therefore, not only is battery performance reduced, but the breakdown voltage of the separator also decreases, leading to high-voltage (hi-pot) failure and low-voltage failure. Therefore, there is a need to develop porous polymer membrane substrates for separators that exhibit minimal deformation even under high-pressure lamination conditions. Summary of the Invention
[0009] Technical issues
[0010] The purpose of this disclosure is to provide a porous substrate for a diaphragm with low thickness deformation rate and high dielectric breakdown voltage, as well as a diaphragm comprising the same. It is apparent that the purpose and advantages of this disclosure can be achieved by the means or methods, or combinations thereof, as described in the claims.
[0011] Technical solution
[0012] This disclosure relates to a porous substrate for a diaphragm, wherein the porous substrate comprises polyethylene and / or polypropylene, the substrate has a porous structure having a plurality of pores, the porosity of the substrate is in the range of 30 vol% to 60 vol%, and the substrate has a pore size distribution, wherein the full width at half maximum (FWHM) of the Gaussian pore distribution, as measured by the pore size distribution, is less than 4.0 nm.
[0013] A second aspect of this disclosure is that, in the first aspect, the FWHM value of the pore distribution is 3.0 nm or less, preferably 2.0 nm or less, and more preferably 1.5 nm or less.
[0014] A third aspect of this disclosure is that, in the first or second aspect, the difference between the maximum pore size (MPs) and the average pore size (mps) is less than 30 nm.
[0015] A fourth aspect of this disclosure is that, in any of the first to third aspects, the difference between the maximum pore size (MPs) and the average pore size (mps) is less than 20 nm.
[0016] The fifth aspect of this disclosure is that, in the third aspect, the average pore size (mps) is in the range of 10 to 100 nm.
[0017] A sixth aspect of this disclosure is that, in the third aspect, the average pore size (mps) is in the range of 20 to 30 nm.
[0018] A seventh aspect of this disclosure is that, in any of the first to sixth aspects, the BET specific surface area of the porous substrate is between 20 and 60 m². 2 Within the range of / g.
[0019] An eighth aspect of this disclosure is that, in any of the first to seventh aspects, the thickness of the porous substrate is in the range of 5 to 20 μm.
[0020] A ninth aspect of this disclosure is that, in any one of the first to eighth aspects, the polymer resin comprises more than 90% by weight of a polyolefin resin relative to 100% by weight of the polymer resin.
[0021] A tenth aspect of this disclosure is that, in any one of the first to ninth aspects, the polydispersity index (PDI) of the polymer resin is in the range of 2.5 to 6.5.
[0022] Furthermore, the eleventh aspect of this disclosure relates to a diaphragm for an electrochemical device, wherein the diaphragm comprises a porous substrate for a diaphragm according to any one of the first to tenth aspects and a heat-resistant layer formed on one or both surfaces of the porous substrate, wherein the heat-resistant layer comprises an adhesive resin and inorganic particles.
[0023] Furthermore, the twelfth aspect of this disclosure relates to an electrochemical device, comprising a negative electrode, a positive electrode, and a diaphragm inserted between the negative electrode and the positive electrode, wherein the diaphragm is the diaphragm according to the eleventh aspect.
[0024] Beneficial effects
[0025] According to this disclosure, the porous substrate has small pore size and uniform pore distribution. When the substrate is used in a diaphragm, the thickness variation is small and the dielectric breakdown voltage is high when the diaphragm and electrodes are laminated together in the lamination process. Attached Figure Description
[0026] The accompanying drawings illustrate preferred embodiments of the present disclosure and, together with the foregoing description of the invention, serve to better understand the technical concept of the present disclosure. Therefore, the present disclosure should not be construed as limited to the content shown in the drawings. Furthermore, the shapes, sizes, scales, or ratios of elements in the drawings included in this specification may be enlarged for clearer emphasis.
[0027] Figure 1 A cross-sectional view of a porous substrate for comparison, and a schematic diagram showing the state of deformation due to compression; Figure 2 This is a cross-sectional view of the porous substrate of the embodiment, and a schematic diagram showing the state of deformation due to compression; Figure 3 An exemplary illustration shows the Gaussian distribution of the holes in the FWHM used to confirm hole dimensions; and Figure 4 Examples are shown of dry sample curves, wet sample curves, and half-dry sample curves obtainable by a porosimeter. Detailed Implementation
[0028] The present disclosure will be described in detail below. Before the description, it should be noted that the terms or words used in this specification and claims should not be interpreted solely based on their conventional or dictionary meanings. The inventor must correctly understand the concept behind each term in order to effectively describe their disclosure. Based on the principle that they can be defined, they should be interpreted as meanings and concepts consistent with the technical ideas of the present disclosure. Therefore, since the configurations described in the embodiments described herein are only the most preferred embodiments of the present disclosure and do not represent the full technical ideas of the present disclosure, it should be understood that various equivalents and variations may exist that can replace them at the time of filing this application.
[0029] Throughout this specification, unless otherwise stated, when a section “contains” a component, it means that it may further contain other components, without excluding other components.
[0030] Furthermore, the terms "about," "substantially," etc., used throughout this specification are interpreted as equal to or close to the stated numerical value when presenting the inherent manufacturing and material tolerances, thereby aiding in the understanding of this application. This is intended to prevent unreasonable infringers from exploiting the disclosure in an unreasonable manner.
[0031] Throughout this specification, the expression "A and / or B" means "A or B or both".
[0032] This disclosure relates to a porous substrate that can be used in membranes for electrochemical devices. In this disclosure, the electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction. It includes the concepts of primary and secondary batteries, wherein the secondary battery is capable of charging and discharging, and includes lithium-ion batteries, nickel-cadmium batteries, nickel-metal hydride batteries, etc.
[0033] diaphragm
[0034] In this specification, the membrane serves as a porous ion-conducting barrier that allows ions to pass through while preventing electrical contact between the negative and positive electrodes in an electrochemical device. Preferably, a plurality of pores are formed in the membrane, and these pores are interconnected, allowing gas or liquid to pass from one side of the membrane to the other.
[0035] According to this disclosure, the diaphragm comprises a porous substrate made of a polymeric material, the porous substrate containing a plurality of pores. If desired, the diaphragm may further comprise an additional layer disposed on at least one surface of the porous substrate, for material or functional purposes. In one embodiment of this disclosure, the diaphragm may comprise the porous substrate and a heat-resistant layer, for example, the heat-resistant layer may be formed on at least one surface of the porous substrate. The heat-resistant layer may contain inorganic particles and a binder resin.
[0036] In one embodiment of this disclosure, the inorganic particles in the heat-resistant layer may be provided in a layered structure, wherein the inorganic particles are bonded by an adhesive resin, and the membrane substrate has a porous structure due to the spaces (interstitial volumes) formed between the inorganic particles. This porous structure has the effect of improving the electrolyte retention capacity of the membrane. On the other hand, in one embodiment of this disclosure, when the membrane includes a heat-resistant layer, the heat-resistant layer accounts for 3% to 40% of the total volume of the membrane when the total volume of the membrane is expressed as 100%. The heat-resistant layer accounts for 5% to 50% of the membrane thickness when the total thickness of the membrane is expressed as 100%.
[0037] Porous substrates
[0038] In one embodiment of this disclosure, the porous substrate may be in the form of a porous sheet comprising a polymer resin and having a plurality of pores. The pores comprise openings, and the openings are interconnected, allowing gas or liquid to pass from one side of the porous substrate to the other. In one embodiment of this disclosure, the air permeability of the porous substrate is preferably less than 2000 sec / 100 ml, and the porosity is preferably 30% to 60% by volume, with respect to battery output and cycle characteristics.
[0039] In this disclosure, air permeability (sec / 100ml) refers to the time, in seconds, required for 100 ml of air to pass through a porous substrate or diaphragm sample, such as one square inch in size, at constant pressure. In one embodiment of this disclosure, air permeability may be measured according to standards in the art. For example, air permeability may be measured using a known Gurley air permeability meter according to ASTM D 726-58 or ASTM D726-94. For instance, air permeability may be 100 ml of air at a pressure of 0.304 kPa or 1.215 kN / m³. 2 Under water pressure, passing through 1 square inch (or 6.54 cm) 2 The time taken to pass through the sample in seconds. According to another embodiment, air permeability can be measured in seconds using the Grie method of Japanese Industrial Standard (JIS-P8117), by measuring the passage of 100 ml of air through a 1 square inch sample at a constant pressure of 4.8 inches of H₂O at room temperature. In one embodiment of this disclosure, air permeability can be measured using, for example, an Asahi Seiko EG01-55-1MR device according to the aforementioned standard.
[0040] Porosity refers to the ratio of the volume occupied by pores to the total volume, expressed in % (volume percentage), and is used interchangeably with terms such as space porosity and multi-porosity. In this disclosure, there are no particular limitations on the measurement of porosity, and methods known in the art can be applied. For example, porosity can be measured using the Brunauer-Emmett-Teller (BET) method with nitrogen, the water intrusion porosimeter method, the capillary flow porosimeter method, or the mercury porosimeter method (Hg porosimeter). Alternatively, in one embodiment of this disclosure, the porosity of a porous substrate can be calculated as the difference between apparent density and net density, wherein the apparent density is obtained by measuring the porous substrate, and the net density of the porous substrate is calculated from the composition ratio of the materials contained in the porous substrate and the density of each component. For example, porosity can be calculated using the following [Formula 1].
[0041] [Formula 1]
[0042] Porosity (volume %) = {1 - (apparent density / net density)} × 100
[0043] On the other hand, the apparent density in the above formula can be calculated by the following [Formula 2].
[0044] [Formula 2]
[0045] Apparent density (g / cm³) 3 = {Weight of porous substrate [g] / (Thickness of porous substrate [cm] × Area of porous substrate [cm²])} 2 ])}
[0046] In this disclosure, the porous substrate has small and uniform pore size, and when applied to diaphragms for electrochemical devices, it exhibits excellent shape stability and dielectric voltage characteristics.
[0047] In this disclosure, the maximum pore size (Mps) of the porous substrate is 80 nm or less, and the difference between the maximum pore size (Mps) and the average pore size (mps) is 30 nm or less, preferably 20 nm or less. Furthermore, the average pore size (mps) is preferably in the range of 10 to 100 nm.
[0048] In one embodiment of this disclosure, the pore size can be calculated from the pore size distribution measured using a capillary flow porosimeter. The capillary flow porosimeter can be used with a porosimeter from Porous Materials Inc. and a Galwick solution, and the measurement method can be described later.
[0049] As a specific example, for each of the porous substrates in a dry state (dry sample) and a wet state (wet sample), a porosity meter is used to measure the relationship between gas pressure and flow rate, and as follows... Figure 4 As shown, ventilation curves for dry samples (dry curve) and wet samples (wet curve) are obtained, and the size and distribution of the pores can be confirmed.
[0050] In capillary flow pore measurement, after wetting a porous substrate with a low-surface-tension wetting solution, the pore size is measured by applying pressure using gas to expel the wetting liquid filling the pores of the porous substrate at the required pressure. For example, after wetting the porous substrate to be measured with a wetting solution such as Galwick solution, the gas pressure on one side of the porous substrate is gradually increased. At this time, when the applied gas pressure is greater than the capillary attraction of the wetting solution present in the pores, the wetting solution blocking the pores is expelled, and the pore size and distribution can be measured by the pressure and flow rate at the time of expulsion. In one embodiment of this disclosure, a non-reactive gas can be used instead of air.
[0051] In one specific embodiment of this disclosure, measurements can be performed within a pressure range of 0 to 3500 MPa, and within this range, the minimum pressure can be above 30 psi and the maximum pressure can be below 500 psi.
[0052] Minimum air pressure can refer to the bubble point pressure. The bubble point is the pressure at the starting point of the pressure curve plotted in a capillary flow porosimeter, and it reflects the largest pore size in the porous substrate. In other words, as the air pressure gradually increases, the wetting solution filling the pores of the diaphragm substrate is pushed by the pressure and moves in order of pore size, thus gradually increasing the airflow rate and eventually drying the sample. Here, the pressure at the starting point of the wetting solution movement is called the bubble point pressure.
[0053] On the other hand, the maximum gas pressure can be the pressure when the sample is finally in a dry state and can reflect the minimum pore size. Alternatively, the maximum gas pressure can be the pressure at the point where the pressure curve (wet curve) of the capillary flow porosity meter measured using the wetting solution intersects with the ventilation curve of the dry sample. The "ventilation curve of the dry sample (dry curve)" is the pressure distribution required to expel the existing gas filling the pores by pressurizing the diaphragm substrate in a dry state without being permeated with the wetting solution using air or a non-reactive gas.
[0054] Figure 4 The wet sample pressure curve and the dry sample pressure curve are displayed using the capillary flow orifice measurement method, and the point where the wet sample pressure curve and the dry sample pressure curve intersect can be the maximum gas pressure.
[0055] On the other hand, in this disclosure, the condition for air under pressure P to enter a hole of diameter D can be expressed by the Washburn formula shown in [Formula 3] below, where the surface tension of the wetting solution is γ and the contact angle of the wetting solution is θ.
[0056] P=(4 γcosθ) / D…(Formula 3)
[0057] Therefore, the diameter of the orifice can be calculated by measuring the pressure when the wetting solution is squeezed out of the orifice.
[0058] On the other hand, when the air flow rate of the wet sample under pressure Pj is Fw,j and the air flow rate of the dry sample is Fd,j, the cumulative filter flow rate (CFF, unit: %) and pore size distribution (PSF: pore size frequency, unit: %) are calculated by Equations 4 and 5, respectively.
[0059] CFF=[(Fw,j / Fd,j)×100] ……(Formula 4)
[0060] PSF = (CFF)j + 1 - (CFF)j ……(Formula 5)
[0061] By combining formulas 3 to 5 above, a pore size distribution curve representing the relationship between pore size D and pore size distribution PSF can be obtained based on the pressure change of airflow under dry and humid conditions. An example of such a pore size distribution curve is shown below. Figure 3 From Figure 3 The aperture distribution curve shown can be used to obtain various physical property values related to the aperture.
[0062] In one embodiment of this disclosure, the bubble point can represent the maximum pore diameter, and the point where the wet sample curve intersects the dry sample curve can represent the minimum pore diameter. Furthermore, the point where the half-dry sample permeability curve (corresponding to half the value of the dry sample permeability curve) intersects the wet sample curve can represent the average pore size (see [link to documentation]). Figure 4 ).
[0063] Furthermore, in this disclosure, the porous substrate exhibits a pore size distribution based on a normal distribution (Gaussian distribution) measured through the pore size distribution (see [reference]). Figure 3 The full width at half maximum (FWHM) in the material is 4.0 nm or less, 2.0 nm or less, or 1 nm or less. Preferably, the FWHM can be 3.0 nm or less. The full width at half maximum (FWHM) is defined as the point at half the maximum value (mode of pore sizes) on the y-axis in a normal distribution of pore size distribution, which is displayed by classifying pores according to their sizes formed within the porous substrate. In this distribution, the x-axis represents the pore size (diameter), and the y-axis represents the frequency (number of pores or percentage of pores, etc.) of the number of pores corresponding to the pore size on the x-axis. In this disclosure, the unit of the x-axis can be expressed in nm or μm. (See reference...) Figure 3 The full width at half maximum (FWHM) can be represented as the difference between two points X2 and X1 on the x-axis, corresponding to half (1 / 2T) of the mode T on the y-axis. This difference can be expressed as an absolute value. On the other hand, the normal distribution can represent symmetric and asymmetric distributions relative to the maximum value, as well as random distributions other than normal.
[0064] In a preferred embodiment of this disclosure, the full width at half maximum (FWHM) can be determined by the distribution of holes other than the largest diameter hole. Alternatively, in this disclosure, the hole shape can be circular, elliptical, or irregular, and the cross-section can be a closed curve. The diameter of the hole refers to the longest distance between any two points on the closed curve. When the above range is satisfied, the porous substrate has small hole sizes and high hole size uniformity. Porous substrates with such characteristics exhibit high shape stability and can demonstrate high dielectric breakdown voltage.
[0065] On the other hand, the BET specific surface area of the porous substrate is preferably between 20 and 60 m². 2Within the range of / g, the larger the BET specific surface area, the higher the porosity and the smaller the pore size. Furthermore, at the same porosity, the smaller the pore size, the larger the BET specific surface area. In this disclosure, the BET specific surface area can be measured using the adsorption formula of the BET (Brunauer, Emmett, and Teller) model, and the adsorption amount can be measured from the measured N2 adsorption isotherm when the adsorption isotherm is measured up to 1 bar (1 atm) at the boiling point temperature of nitrogen (-196 °C).
[0066] In this disclosure, the thickness of the porous substrate can be in the range of 5 to 20 μm for the purposes of thinning and increasing the energy density of the electrochemical device. When the thickness of the porous substrate is less than the above range, the function of the conductive barrier is insufficient, while when the thickness exceeds the above range (i.e., too thick), the resistance of the membrane may increase excessively.
[0067] On the other hand, in one embodiment of this disclosure, from the viewpoint of imparting a closed-cell function, the polymer resin may comprise a thermoplastic resin with a melting point of less than 200°C, and preferably may comprise at least one of polyolefin resins. The closed-cell function refers to the function of preventing battery thermal runaway by blocking the movement of ions between the positive and negative electrodes by melting the polymer resin to close the pores of the porous substrate when the battery temperature is high.
[0068] Examples of the polyolefin resin may include polyethylene, polypropylene, polybutene, polypentene, etc., and may include one or more mixtures thereof. As a specific example, the polyolefin resin may include two or more selected from polyethylene, polypropylene, and polypentene. In another example, the polyolefin resin may be polyethylene and / or polypropylene.
[0069] In one specific embodiment of this disclosure, the porous substrate comprises a polyethylene substrate, and may additionally comprise polypropylene if desired. In this case, the polypropylene content is 0% to 5% by weight relative to 100% by weight of the substrate. For example, the polypropylene content may be less than 5% by weight. On the other hand, in one embodiment of this disclosure, for achieving the compression ratio range described later, the weight-average molecular weight (Mw) of the polyethylene may be in the range of 300,000 to 1,800,000 g / mol, preferably 300,000 to 1,500,000 g / mol, or 3,000,000 to 1,000,000 g / mol, or 300,000 to 500,000 g / mol.
[0070] On the other hand, in this disclosure, the content of the polyolefin resin is preferably 90% by weight or more or 95% by weight or more relative to 100% by weight of polymer material.
[0071] Examples of the polyolefin resin may include one or more mixtures selected from the group consisting of polyethylene, polypropylene, polybutene, and polypentene. Specifically, the polyolefin resin may be polyethylene and / or polypropylene.
[0072] On the other hand, in one specific embodiment of this disclosure, the polydispersity index (PDI) value of the polymer resin is preferably in the range of 2.5 to 6.5. In one embodiment, when two or more types of polymer resins are mixed, the mixed polymer resin can satisfy the PDI. In a more preferred embodiment, relative to 100% of the polymer resin satisfying the above-mentioned PDI range, any type of polymer resin as a single component accounts for more than 50%, 70% by weight or more, or 90% by weight or more. The polymer resin may consist of only a single component. The single component refers to polymer resins with the same chemical structure (especially repeating units) and a PDI in the range of 2.5 to 6.5.
[0073] In one specific embodiment of this disclosure, the polymer material may contain more than 90% by weight of polyethylene with a PDI of 2.5 to 6.5.
[0074] As described above, when the PDI value or the content range of the polymer resin is met, the uniformity in terms of the size and distribution of pores in the polymer substrate can be improved. On the other hand, the polydispersity index can be obtained from the ratio of number-average molecular weight (Mn) to weight-average molecular weight (Mw).
[0075] On the other hand, in this disclosure, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be measured by gel permeation chromatography (GPC) (PL GPC220, Agilent Technologies), and the measurement conditions can be set as follows.
[0076] - Column: PL Olexis (Polymer Laboratories Co.)
[0077] - Solvent: TCB (trichlorobenzene)
[0078] - Flow rate: 1.0 ml / min
[0079] - Sample concentration: 1.0 mg / ml
[0080] Injection volume: 200 μl
[0081] - Column temperature: 160℃
[0082] - Detector: Agilent High Temperature RI Detector
[0083] - Standard: Polystyrene (corrected using a cubic function)
[0084] In another embodiment, the melt index (MI) of the polymer material can be in the range of 0.02 to 1.0 g / 10 minutes. The MI is based on the condition of applying a 21.6 kg load at 190°C.
[0085] In one embodiment of this disclosure, the porous substrate may contain polypropylene, but it is preferred that the polypropylene content in the porous substrate be controlled to be less than 5% by weight, for example, less than 5% by weight. Higher polypropylene content results in lower polymer crystallinity. Therefore, even with high porosity and low permeability, compressibility or permanent deformation is not reduced, and the withstand voltage defect rate, as a dielectric characteristic, can be kept at a low level. However, if the polypropylene content exceeds the recommended range while preparing the porous substrate using a wet process, the raw material may become chemically unstable and hinder proper pore formation. That is, this is disadvantageous in terms of the performance of porous properties, and it is preferable to control the polypropylene content within the aforementioned range.
[0086] Furthermore, when the polypropylene content is high, it is easier to manufacture using the dry method than the wet method, thereby obtaining a porous substrate with well-developed pores. However, when using the dry manufacturing method, it is more difficult to control the thickness of the porous substrate to be thinner compared to using the wet manufacturing method.
[0087] On the other hand, in one specific embodiment of this disclosure, the porous substrate may further comprise at least one of the following polymer resins: polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, and polyethylene naphthalate.
[0088] In one embodiment of this disclosure, a porous substrate of polymer material satisfying the above-mentioned thickness range can be prepared by means of a wet manufacturing method using polyethylene.
[0089] On the other hand, in one specific embodiment of this disclosure, the porous substrate may be a porous polymer membrane prepared in a manner described later, and may be a single-layer membrane or a multilayer membrane formed by laminating two or more sheets.
[0090] In this disclosure, the separator that meets the above values improves the dielectric voltage characteristics of the battery, resulting in an increase in breakdown voltage and a decrease in short-circuit incidence (voltage failure rate) even under high voltage conditions.
[0091] On the other hand, in this disclosure, dielectric breakdown voltage is the highest voltage that an insulator can withstand, and dielectric breakdown refers to the destruction of an insulator and loss of its insulating properties when a voltage is applied to it and the voltage exceeds a certain value.
[0092] In one embodiment of this disclosure, the dielectric voltage characteristics can be confirmed by measuring the dielectric breakdown voltage of the diaphragm, which is an insulator, by placing a diaphragm between two conductors and applying a voltage to measure the voltage at which dielectric breakdown occurs.
[0093] The dielectric breakdown voltage can be measured, for example, using an AC / DC / IR Hi-Pot tester. For instance, a stainless steel mesh and a porous substrate are hot-pressed together at 90°C, 4 MPa, and 1 second, then a DC current is set to 0.5 mA and boosted to 100 V / s (3 kV voltage, 3 s rise time). The measurement is completed when a short circuit occurs as the voltage increases, and this voltage is defined as the dielectric breakdown voltage.
[0094] Furthermore, in one embodiment of this disclosure, the evaluation of the withstand voltage defect rate can be measured by determining, through Weibull analysis, the voltage represented by the lower 1% of samples exhibiting low dielectric breakdown voltage out of the total number of tested samples.
[0095] Methods for preparing porous substrates
[0096] In one embodiment of this disclosure, the porous substrate can be prepared by a method for producing a polymer film, preferably a wet process. For example, the wet manufacturing method includes preparing a mixture S1, extruding the mixture to form an extruded sheet S2, stretching the extruded sheet S3, removing the pore-forming agent S4, and heat-setting the extruded sheet S5.
[0097] In step S1, the type of polymer resin is appropriately selected considering the final physical properties of the membrane, and the selected polymer resin is mixed with a pore-forming agent. The polymer resin may refer to the aforementioned porous substrate polymer resin. For example, the polymer resin may be a polyolefin polymer resin. Examples of polyolefin polymer resins may include one or more polymers selected from polyethylene such as high-density polyethylene, linear low-density polyethylene, low-density polyethylene, or ultra-high molecular weight polyethylene, polypropylene, polybutene, and polypentene, or combinations thereof.
[0098] The pore-forming agent is a material dispersed in the polymer, exhibiting heterogeneity in the substrate prepared by extrusion, stretching, etc., and subsequently removed from the substrate. Therefore, the substrate portion containing the pore-forming agent retains the pore form of the substrate. The pore-forming agent is preferably a liquid material in the extrusion process, but materials that remain solid can also be used. The pore-forming agent can be an aliphatic hydrocarbon solvent, such as liquid paraffin, paraffin oil, mineral oil, or paraffin; vegetable oils, such as soybean oil, sunflower oil, rapeseed oil, palm oil, coconut oil, corn oil, grapeseed oil, cottonseed oil, etc.; or a plasticizer, such as dialkyl phthalates. Specifically, the plasticizer can be di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), butyl benzyl phthalate (BBP), etc. Liquid paraffin (LP, also known as "liquid paraffin") is particularly preferred.
[0099] Furthermore, the content of the pore-forming agent during membrane preparation can be appropriately adjusted to achieve the desired porosity level. While a high content of pore-forming agent is preferred for improving air permeability, excessive pore-forming agent content can adversely affect the strength of the final substrate. Therefore, the content of the pore-forming agent can be from 1% to 80% by weight relative to 100% of the total polymer resin and pore-forming agent. Depending on the requirements, it can be adjusted to 70% or less, 60% or less, or 50% or less within the above range, and can be adjusted to more than 1% by weight, more than 20% by weight, or more than 40% by weight. On the other hand, in one specific embodiment of this disclosure, for example, to achieve a porosity of about 45% or less in the porous substrate, the pore-forming agent can be included in the range of 1% to 60% by weight relative to 100% of the total polymer resin and pore-forming agent.
[0100] Next, the mixture prepared in the above steps is extruded using an extruder to obtain an extruded sheet. There are no particular limitations on the extruder, and any extruder commonly used in the art can be used, such as, but not limited to, extruders with T-die or tubular dies. Although the extrusion process can be carried out at conventional extrusion temperatures, it is preferred to carry out the extrusion process at a temperature 10°C to 100°C higher than the melting point of the polymer resin used. When the extrusion process exceeds this range excessively, the polymer resin undergoes thermal decomposition, making film formation difficult and reducing the physical properties of the manufactured substrate, which is not preferred. An extruded sheet can be obtained through this extrusion process.
[0101] The extruded sheet is then fed into a stretching process. This stretching process is performed using a stretching machine commonly used in the art. The stretching machine can be a sequential biaxial stretching machine, but is not particularly limited thereto. By stretching the extruded sheet in this manner, the mechanical strength of the porous substrate can be increased. The stretching process is performed in the machine direction (MD, longitudinal direction) and / or the transverse direction (TD, vertical direction). Stretching in all or one of these directions increases the tensile strength in the respective stretching direction. If desired, the diaphragm of this disclosure can be manufactured by performing longitudinal (MD) stretching and / or transverse (TD) stretching separately in one direction during the stretching process (e.g., uniaxial stretching), or by performing stretching simultaneously or sequentially in both directions (e.g., biaxial stretching). On the other hand, in one embodiment of this disclosure, the temperature of the stretched film can be controlled to 100°C to 130°C, preferably 110°C to 125°C. For example, the temperature of the film during stretching can be controlled in the range of 115°C to 121°C. When the stretching process is performed within the above temperature range, a membrane with small and uniform pores can be obtained.
[0102] Next, the pore-forming agent is removed from the extruded sheet obtained above. The pore-forming agent is removed by solvent extraction and drying. Furthermore, through this removal process, the spaces occupied by the pore-forming agent are formed into pores. The solvent that can be used to extract the pore-forming agent can be any solvent capable of extracting pore-forming agents. Nevertheless, it is suitable to use solvents with high extraction efficiency and fast drying, such as methyl ethyl ketone, dichloromethane, and hexane. Preferably, the solvent can be dichloromethane (MC), such as methylene dichloride. As extraction methods, all commonly used solvent extraction methods, such as impregnation, solvent spraying, and ultrasonic methods, can be used alone or in combination.
[0103] After the extraction of the pore-forming agent, the substrate is heat-set to ultimately obtain a membrane with the desired physical properties, porosity, and permeability. The heat-setting step can be performed using a heating device, such as an oven, capable of applying the appropriate temperature required for heat setting. Specifically, to reduce shrinkage of the final membrane by removing residual stress, the pre-dried membrane is heat-set as a final step. Heat setting removes residual stress by applying heat while simultaneously fixing the membrane to force it to hold. Higher heat-setting temperatures are beneficial for reducing shrinkage, but if the temperature is too high, the membrane may partially melt, clogging the formed pores and reducing permeability. The heat-setting temperature is preferably selected within the range where approximately 10% to 30% of the membrane crystals melt. If the selected heat-setting temperature is lower than the temperature at which approximately 10% by weight of the membrane crystals melt, the reorientation of polyethylene molecules in the membrane is insufficient, and there is no effect on removing residual stress from the membrane. If the selected heat setting temperature is higher than the temperature at which approximately 30% by weight of the film crystallization melts, the pores will become clogged due to partial melting, thereby reducing air permeability.
[0104] In one embodiment of this disclosure, the porous substrate may be a single layer. Alternatively, the porous substrate may be a laminate in which two or more films are stacked. In this case, at least one of the films included in the laminate may be formed by the method described above.
[0105] heat-resistant layer
[0106] In one embodiment of this disclosure, the diaphragm may include a heat-resistant layer formed on at least one surface of a porous substrate. The heat-resistant layer comprises an adhesive resin and inorganic particles, and has a plurality of micropores within it, with the structure of the heat-resistant layer such that these micropores are interconnected. The heat-resistant layer is structurally unique in that it is a porous layer that allows gas or liquid to pass through from one side to the opposite side. In one embodiment of this disclosure, the heat-resistant layer may contain adhesive resin and inorganic particles in a weight ratio of 1:99 to 30:70. This ratio can be suitably adjusted within the above range; for example, when the sum of the adhesive resin and inorganic particles is 100% by weight, the adhesive resin may be 1% or more by weight, 5% or more by weight, or 10% or more by weight, and the inorganic particles may be 80% or more by weight, 85% or more by weight, 90% or more by weight, or 95% or more by weight. In this disclosure, from the viewpoint of ion permeability, it is preferable that the heat-resistant layer has a porous structure.
[0107] In the heat-resistant layer, inorganic particles are bonded together by an adhesive resin, and pores can be formed due to the interstitial volume between the inorganic particles. This interstitial volume is the space defined by the inorganic particles, which are essentially arranged in a close-packed or densely packed structure facing each other.
[0108] In one embodiment of this disclosure, the porosity of the heat-resistant layer can be from 30 vol% to 70 vol%, and within this range, the porosity can be simultaneously or independently 35 vol% or more, 40 vol% or more, and 65 vol% or less or 60 vol% or less. For example, the porosity can be in the range of 40 vol% to 60 vol%. When the porosity is below 70 vol%, it can be ensured that the mechanical properties of the pressurization process performed to bond the diaphragm to the electrode can be withstood, and the surface opening ratio will not increase to an excessively high level. Therefore, a porosity of below 70 vol% is suitable for obtaining good adhesion. On the other hand, when the porosity is above 30 vol%, it is advantageous in terms of ion permeability.
[0109] In this disclosure, the porosity can be measured using an adsorbed gas such as nitrogen and a BELSORP (BET device) manufactured by Bayer Japan, or by a method such as a mercury porosimeter. Alternatively, in one embodiment of this disclosure, the net density of the electrode active material layer is calculated based on the density (apparent density) of the obtained electrode (electrode active material layer), the content ratio of the materials contained in the electrode (electrode active material layer), and the density of each component of the electrode active material layer. Furthermore, the porosity of the electrode active material layer can be calculated from the difference between the apparent density and the net density.
[0110] The thickness of the heat-resistant layer on one side of the porous substrate can be in the range of 1 to 6 μm. Within this range, if desired, the thickness of the heat-resistant layer can be 2 μm or more, or 3 μm or more. Within this numerical range, adhesion to the electrode is excellent, resulting in increased battery strength. On the other hand, a thickness of 6 μm or less is advantageous in terms of battery cycle characteristics and resistance characteristics. From this perspective, a thickness of 4 μm or less is preferred, and more preferably 3 μm or less.
[0111] In this disclosure, non-limiting examples of adhesive resins that can be used for heat-resistant layers may include at least one polymer resin selected from the group consisting of: polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polymethyl methacrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose, or mixtures of two or more thereof. However, this disclosure is not specifically limited thereto.
[0112] In one specific embodiment of this disclosure, the inorganic particles that can be used in the heat-resistant layer are not particularly limited, as long as they are electrochemically stable. That is, there are no particular limitations on the inorganic particles that can be used in this disclosure, as long as they are within the operating voltage range of the applied electrochemical device (e.g., based on Li / Li). + As long as there is no oxidation and / or reduction reaction (at 0 to 5V).
[0113] Non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0<x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 The inorganic particles may include one or more of the following: PbTiO3 (PMN-PT), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), zinc tin oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), and antimony pentoxide (Sb2O5).
[0114] Independently or in combination with the components of the examples above, the inorganic particles may comprise inorganic particles with lithium-ion transport capabilities. Non-limiting examples of such inorganic particles with lithium-ion transport capabilities may include lithium phosphate (Li3PO4), lithium titanium phosphate (Li... x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0<x<2, 0<y<1, 0<z<3), (LiAlTiP) x O y Glass (0 < x < 4, 0 < y < 13) such as 14Li₂O-9Al₂O₃-38TiO₂-39P₂O₅, lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0<x<4, 0<y<1, 0<z<1, 0<w<5) as Li3.25 Ge 0.25 P 0.75 S4, lithium nitrides (Li x N y (0 < x < 4, 0 < y < 2) such as Li3N, SiS2 glass (Li x Si y S z (0 < x < 3, 0 < y < 2, 0 < z < 4) such as Li3PO4-Li2S-SiS2, P2S5 series glass (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) such as LiI-Li2S-P2S5, or mixtures thereof.
[0115] Furthermore, the average diameter (D) of the inorganic particles 50 There are no particular limitations, but in order to form a coating with uniform thickness and appropriate porosity, a range of 0.3 to 1 μm is preferred. When the average diameter of the inorganic particles is less than 0.3 μm, the dispersibility of the inorganic particles in the prepared heat-resistant layer slurry may decrease, and when the average diameter of the inorganic particles is greater than 1 μm, the thickness of the formed coating may increase.
[0116] In one embodiment of this disclosure, the method for forming the heat-resistant layer is as follows. First, a polymer solution is prepared by dissolving the adhesive resin in a suitable organic solvent. Preferably, the solubility parameter of the solvent is similar to that of the adhesive polymer to be used, and it has a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of solvents that can be used include acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or mixtures thereof.
[0117] Subsequently, inorganic particles are added and dispersed in the prepared polymer solution. In this disclosure, the ratio of inorganic particles to binder is as described above and is appropriately adjusted taking into account the thickness, pore size, and porosity of the heat-resistant layer of the final manufactured product.
[0118] Next, the inorganic particle slurry prepared above is applied to at least one side of the diaphragm and dried. There are no particular limitations on the method of applying the slurry to the diaphragm substrate, and conventional coating methods known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.
[0119] During the drying process, temperature and time conditions are appropriately set to minimize surface defects on the composite porous layer surface. Drying can be carried out using appropriate drying aids such as drying ovens or hot air.
[0120] Furthermore, the diaphragm of this disclosure can also be manufactured by methods in which a heat-resistant layer and a porous substrate are prepared separately, and the sheets are overlapped and combined by hot pressing or adhesion. Examples of methods for obtaining a heat-resistant layer as an independent sheet include methods in which a slurry is applied to a release sheet, a heat-resistant layer is formed by the above methods, and only the heat-resistant layer is peeled off.
[0121] On the other hand, this disclosure provides a secondary battery including a separator. The battery includes a negative electrode, a positive electrode, and a separator interposed between the negative electrode and the positive electrode, and the separator is a low-resistance separator having the aforementioned characteristics.
[0122] In this disclosure, the positive electrode comprises a positive current collector and a positive active material layer on at least one surface of the current collector, the positive active material layer comprising a positive active material, a conductive material, and a binder resin. The positive active material may comprise one or a mixture of two or more layered compounds, such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or compounds substituted with one or more transition metals; Li 1+x Mn 2-x Lithium manganese oxides of O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, LiV3O4, V2O5 and Cu2V2O7; and LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x = 0.01 to 0.3); LiMn 1- x M x Lithium manganese composite oxides represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); LiMn2O4, wherein a portion of the Li in the formula is replaced by an alkaline earth metal ion; disulfide compounds; and Fe2(MoO4)3.
[0123] In this disclosure, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer on at least one surface of the current collector, the negative electrode active material layer comprising a negative electrode active material, a conductive material, and a binder resin. The negative electrode may contain at least one component or a mixture of two or more components selected from the group consisting of: lithium metal oxide; carbon, such as non-graphitized carbon and graphitic carbon; metal composite oxides, such as Li... x Fe2O3 (0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements in Groups 1, 2, and 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloys; silicon alloys; tin alloys; metal oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers, such as polyacetylene; Li-Co-Ni materials; and titanium oxides.
[0124] In one specific embodiment of this disclosure, the conductive material may be, for example, any one selected from the group consisting of: graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whiskers, conductive metal oxide, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials. More specifically, the conductive material may be one selected from the group consisting of: natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal cracking black, tantalizer black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more of these conductive materials.
[0125] There are no particular restrictions on the current collector, as long as it has high conductivity and does not cause chemical changes in the battery. For example, stainless steel, copper, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel materials with surface treatments such as carbon, nickel, titanium, and silver can be used.
[0126] As the adhesive resin, polymers commonly used in the art for electrodes can be used. Non-limiting examples of such adhesive resins may include, but are not limited to, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polymethyl methacrylate, ethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-vinyl acetate copolymer, polyethylene oxide, polyarylates, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxymethyl cellulose.
[0127] The electrode assembly prepared as described above can be housed in a suitable casing and injected with electrolyte to manufacture a battery.
[0128] In this disclosure, the electrolyte comprises substances having the same properties as A. + B - Salts with the same structure, and A + Including ions formed from alkali metal cations, such as Li + Na + K + or a combination thereof, and B - Including PF6 - BF4 - Cl - ,Br - I - ClO4 - AsF6 - CH3CO2 - CF3SO3 - N(CF3SO2)2 - C(CF2SO2)3 - Or a combination thereof. In this electrolyte, the salt may be soluble or dissociated in an organic solvent comprising or a mixture thereof: propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone (γ-butyrolactone), but not limited thereto.
[0129] Furthermore, this disclosure provides a battery module, a battery pack including the battery module, and a device including the battery pack as a power source. The battery module includes a battery, and the battery includes the aforementioned electrode assembly as a unit cell. Specific examples of the device include power tools driven by a battery motor; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), etc.; electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and energy storage systems, but are not limited thereto.
[0130] Hereinafter, embodiments will be given to describe the present disclosure in detail. However, embodiments of the present disclosure may be modified in various other ways, and the scope of the present disclosure should not be construed as limited to the embodiments described later. Embodiments of the present disclosure are provided to explain the present disclosure more fully to those skilled in the art.
[0131] [Example]
[0132] 1. Preparation of porous substrates
[0133] [Example 1]
[0134] 30 parts by weight of polyethylene resin (Mw 475500 g / mol, PDI 3.6) and 70 parts by weight of liquid paraffin oil (dynamic viscosity at 40°C: 40 cSt) were kneaded and then extruded in a twin-screw extruder. After extrusion, the extruded material was passed through a T-die and a cooling casting roller to form a sheet, which was then biaxially stretched using a tenter frame type simultaneous stretching machine that performs MD stretching followed by TD stretching. The liquid paraffin oil, used as a diluent, was extracted from the stretched sheet with dichloromethane and heat-set at approximately 128°C to obtain a porous substrate for diaphragms.
[0135] [Example 2]
[0136] 30 parts by weight of polyethylene resin (Mw 930800 g / mol, PDI 3.3) and 70 parts by weight of liquid paraffin oil (dynamic viscosity at 40°C: 40 cSt) were kneaded and then extruded in a twin-screw extruder. After extrusion, the extruded material was passed through a T-die and a cooling casting roller to form a sheet, which was then sequentially stretched (MD stretching + TD stretching) using a tenter frame. The liquid paraffin oil, used as a diluent, was extracted from the stretched sheet with dichloromethane and heat-set at approximately 128°C to obtain a porous substrate for diaphragms.
[0137] [Comparative Example 1]
[0138] A polyethylene resin composition was prepared by mixing a first polyethylene resin (weight-average molecular weight (Mw) of 250,000 g / mol) and a second polyethylene resin (weight-average molecular weight (Mw) of 800,000 g / mol). The composition had a molecular weight (Mw) of 497,000 g / mol and a PDI of 12.8. Next, a porous substrate for a membrane was obtained in the same manner as in the above examples.
[0139] [Comparative Example 2]
[0140] A polyethylene resin composition was prepared by mixing a first polyethylene resin (weight-average molecular weight (Mw) of 250,000 g / mol) and a second polyethylene resin (weight-average molecular weight (Mw) of 800,000 g / mol). The composition had a molecular weight (Mw) of 381,000 g / mol and a PDI of 10.5. Next, a porous substrate for a diaphragm was obtained in the same manner as in the above examples.
[0141] The porous substrates obtained in each embodiment and comparative example are summarized in Table 1 below.
[0142] [Table 1]
[0143] 2. Evaluation of the physical properties of porous substrates
[0144] (1) Regarding the distribution of hole size
[0145] Samples with dimensions of 5 cm in the TD direction and 5 cm in the MD direction were obtained at the central portion of the porous substrates obtained in the various embodiments and comparative examples. For each obtained sample, a dry curve was obtained using a Perm-Porometer (CFP-1500A) manufactured by Porous Materials Corporation (PMI). Furthermore, a wet curve was obtained after filling the porous substrate with Galwick solution. Measurement pressures ranged from 0 to 3500 MPa. The maximum pore size (MPs), average pore size (mps), full width at half maximum (FWHM), and the difference between the maximum pore size (MPs) and the average pore size (mps) were calculated. Furthermore, the calculated pore size distribution results are shown below. Figure 3 middle.
[0146] In the obtained curves, the bubble point represents the maximum pore diameter, and the intersection of the wet sample curve and the dry sample curve represents the minimum pore diameter. Furthermore, the intersection of the half-dry sample permeability curve (corresponding to half the value of the dry sample permeability curve) and the wet sample curve represents the average pore size (see [link to curve]). Figure 4 ).
[0147] (2) BET specific surface area measurement
[0148] When the adsorption isotherms of the porous substrates obtained in the examples and comparative examples were measured up to 1 bar using a BET surface area analyzer (BEL, Microtrac Co., USA) at -196°C, the BET surface area was calculated from the measured N2 adsorption isotherms using the Brunol-Emmett-Teller model (BET).
[0149] (3) Porosity measurement
[0150] Porosity is calculated using the following [Formula 1] and [Formula 2].
[0151] [Formula 1]
[0152] Porosity (volume %) = {1 - (apparent density / net density)} × 100
[0153] [Formula 2]
[0154] Apparent density (g / cm³) 3 = {Weight of porous substrate [g] / (Thickness of porous substrate [cm] × Area of porous substrate [cm²])} 2 ])}
[0155] Three samples with a dimension of 5 cm in the MD / TD direction were obtained from the porous substrates of the various embodiments and comparative examples. For the thickness of the porous substrate, the average value was used after measuring five points on each sample, and the weight of each sample was measured using a balance. The average value of the three samples was calculated and substituted into Formulas 1 and 2 above to calculate the porosity. On the other hand, the net density in each sample was applied based on theoretically confirmed values (e.g., the molecular weight of each applied component).
[0156] (4) Measurement of air permeability and rate of change of air permeability
[0157] The air permeability of the porous substrates obtained in each embodiment and comparative example was confirmed. The air permeability was measured using an air permeability tester EG01-55-1MR manufactured by Asahi Seiko Co., Ltd., according to the Fraser test method of ASTM D 737.
[0158] [Air permeability tester device settings]
[0159] Measurement pressure: 0.5 kg / cm 2 Cylinder pressure: 2.5 kg / cm² 2 Time setting: 10 seconds
[0160] At least 10 samples were extracted from the porous substrates obtained from each embodiment and comparative example, and the average value of the data was described.
[0161] On the other hand, after hot-pressing each porous substrate at 90°C, 4 MPa and 1 second, the air permeability was measured, and the air permeability change rate (%) of each porous substrate was calculated by Equation 3 below.
[0162] [Formula 3]
[0163] [(Initial air permeability - Air permeability after compression) / Initial air permeability] × 100
[0164] (5) Thickness change rate
[0165] The initial thickness and the thickness after pressing of the porous substrate were measured using a contact thickness gauge. Measurements were taken at 5 mm intervals within a 30 cm distance along the TD direction of the porous substrate. Five measurements were taken along the TD direction at different MD locations, and the arithmetic mean was taken as the thickness of the porous substrate. On the other hand, the thickness change rate (%) of each porous substrate was calculated using the following [Equation 4].
[0166] [Formula 4]
[0167] [(Initial thickness - Post-pressed thickness) / Initial thickness] × 100
[0168] It has been confirmed that the thickness change rate of the porous substrate in Example 1 is lower than that of the porous substrates in Comparative Examples 1 and 2.
[0169] (6) Dielectric breakdown voltage
[0170] Thirty samples were prepared for each example and comparative example, and their dielectric voltage characteristics were evaluated. After hot-pressing a stainless steel mesh and a porous substrate at 90°C, 4 MPa, and 1 second, a DC current was set to 0.5 mA and the voltage was boosted to 100 V / s (3 kV voltage, 3 s rise time). The voltage was increased at the start of the experiment and measured when a short circuit occurred in each sample; this voltage was then taken as the breakdown voltage. The voltages of the lower 1% of the tested samples exhibiting low breakdown voltages were measured using Weibull analysis, and these are summarized in Table 1.
[0171] As confirmed in the experiment, compared with the porous substrate according to the comparative example, the porous substrate according to the embodiment has smaller and more uniform pore size, resulting in superior dielectric voltage characteristics and thickness variation rate.
[0172] (7) Measurement of polydispersity index
[0173] The multi-dispersion index is calculated according to Equation 5 below.
[0174] [Formula 5]
[0175] Polydispersity index = weight-average molecular weight (Mw) / number-average molecular weight (Mn)
[0176] Weight-average molecular weight (Mw) and number-average molecular weight (Mn) were measured by gel permeation chromatography (GPC) (PLGPC220, Agilent Technologies), and the measurement conditions could be set as follows.
[0177] - Column: PL Olexis (Polymer Labs)
[0178] - Solvent: TCB (1,2,4-trichlorobenzene, Wako Pure Chemical Industries, Ltd.)
[0179] - Flow rate: 1.0 ml / min
[0180] - Sample concentration: 1.0 mg / ml
[0181] - Injection volume: 200 μl
[0182] - Column temperature: 160℃
[0183] - Detector: Agilent High Temperature RI Detector
[0184] - Standard: Polystyrene (corrected using a cubic function)
Claims
1. A porous substrate for a diaphragm, said porous substrate comprising a polyolefin polymer resin, The polymer resin comprises polyethylene and / or polypropylene, and The substrate has a porous structure, and the porous structure has multiple pores. The porosity of the substrate is in the range of 30 to 60% by volume, and The substrate has a pore size distribution, wherein the full width at half maximum (FWHM) of the Gaussian pore distribution, as measured by the pore size distribution, is less than 3.0 nm. The difference between the maximum pore size and the average pore size is less than 30 nm. The average pore size is in the range of 10 to 100 nm, and The polydispersity index of the polymer resin is in the range of 2.5 to 6.
5.
2. The porous substrate for a diaphragm according to claim 1, wherein the full width at half maximum (FWHM) of the pore size distribution is less than 2.0 nm.
3. The porous substrate for diaphragms according to claim 1, wherein the difference between the maximum pore size and the average pore size is less than 20 nm.
4. The porous substrate for a diaphragm according to claim 1, wherein the average pore size is in the range of 20 to 30 nm.
5. The porous substrate for a diaphragm according to claim 1, wherein the BET specific surface area of the porous substrate is between 20 and 60 m². 2 Within the range of / g.
6. The porous substrate for a diaphragm according to claim 1, wherein the thickness of the porous substrate is in the range of 5 to 20 μm.
7. The porous substrate for a diaphragm according to claim 1, wherein the polymer resin comprises 90% or more polyolefin resin relative to 100% by weight of the polymer resin.
8. A diaphragm comprising a porous substrate for a diaphragm according to any one of claims 1 to 7 and a heat-resistant layer formed on one or both surfaces of the porous substrate. The heat-resistant layer comprises an adhesive resin and inorganic particles.
9. An electrochemical device comprising a negative electrode, a positive electrode, and a membrane disposed between the negative electrode and the positive electrode, wherein the membrane is the membrane according to claim 8.
Citation Information
Patent Citations
Battery separator and its manufacture
JP1999329390A
Deep learning-based management method of unmanned store system using high performance computing resources
KR1020210059551A
Separator for electricity storage devices, and electricity storage device
CN111201635A
Microporous film and separator using the same
JP2015120786A
Separator with heat resistant insulation layer
US20140287295A1