A recycled concrete resistant to hydration thermal cracking

The combination of modified recycled aggregate and non-calcined shell powder solves the problems of low early tensile strength of recycled concrete and cracks caused by hydration heat, improves the tensile strength and anti-permeability of concrete, and ensures the durability of large concrete bodies. Stability and aesthetics.

CN116496043BActive Publication Date: 2024-10-25CHONGDE BUILDING MATERIALS GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310435720.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-22
Publication Date
2024-10-25
Estimated Expiration
2043-04-22

AI Technical Summary

Technical Problem

Existing recycled concrete has low early tensile strength when used in large concrete bodies, and is easily affected by hydration heat to cause cracks, affecting the appearance and anti-permeability.

Method used

Modified regenerated aggregate and non-calcined shell powder are used, and the regenerated aggregate is activated by alkali solution to form a high-strength surface gel to reduce water absorption, and plant fiber silk is added to enhance the anti-cracking performance.

Benefits of technology

It improves the early tensile strength of recycled concrete, reduces the occurrence of cracks, enhances permeability resistance, and ensures the appearance and performance of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to environmentally friendly building materials, and specifically discloses a recycled concrete that is resistant to hydration heat cracking, which solves the problem that the recycled concrete has low early strength and is easily cracked due to hydration heat when used on large concrete bodies. The application specifically includes: a recycled concrete that is resistant to hydration heat cracking, comprising the following raw materials in parts by mass: 200-400 parts of natural aggregate; 600-800 parts of modified recycled aggregate; 350-420 parts of cement; 400-480 parts of sand; 120-156 parts of non-calcined shell powder; the modified recycled aggregate is obtained by activating the recycled aggregate mixed with alkali solution; the recycled concrete of the application uses the modified recycled aggregate and the non-calcined shell powder of the application at the same time, and the two work synergistically to improve the recycled aggregate, improve the bonding performance of cement mortar without affecting the natural aggregate, and ultimately improve the early tensile strength of the recycled concrete and reduce the possibility of cracking of the recycled concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of environmentally friendly building materials, and more specifically, to recycled concrete resistant to hydration thermal cracking. Background Art

[0002] Recycled concrete is concrete that uses materials obtained from crushing old concrete as part of its raw materials, turning original construction waste into treasure, improving resource utilization and reducing environmental pollution.

[0003] The more common way now is to screen the broken pieces of old concrete and take the old aggregate blocks as recycled aggregate to replace or partially replace natural aggregate. Recycled aggregate is subjected to mechanical pressure during the crushing process, and has more cracks and damage than natural aggregate, and is not as strong as natural aggregate. Therefore, recycled aggregate is avoided as much as possible in high-load-bearing concrete bodies such as bridge piers in actual application, and is more commonly used in low-strength concrete bodies, and the cost is greatly reduced.

[0004] However, during actual use, the inventors of this application found that when recycled concrete is used in some low-strength, large-volume concrete bodies such as walls, retaining dams, cast curbs, large flower beds, and pool walls, the initial strength of the concrete after pouring is low due to the poor bonding between the recycled aggregate and the new cement slurry. At the same time, the recycled aggregate absorbs a large amount of water, the hydration heat is severe during concrete curing, and the temperature difference between the inside and outside of the concrete body is severe. Under the influence of low early strength and high hydration heat, this type of concrete body often develops cracks, affecting the appearance and anti-permeability of the concrete body. Summary of the invention

[0005] In order to solve the problem that the existing recycled concrete has low early tensile strength and is prone to cracking due to hydration heat when used on large concrete bodies, the present application provides a recycled concrete that is resistant to hydration heat cracking, which specifically adopts the following technical solution: A recycled concrete that is resistant to hydration heat cracking, comprising the following raw materials in parts by mass:

[0006] 200-400 parts of natural aggregate;

[0007] 600-800 parts of modified recycled aggregate;

[0008] 350-420 parts of cement;

[0009] 400-480 parts of sand;

[0010] 120-156 parts of non-calcined shell powder;

[0011] The modified recycled aggregate is obtained by activating the recycled aggregate mixed with alkali solution, the alkali solution is prepared by one or more of NaOH, KOH, and Ca(OH)2, and the amount of the alkali solution is 50 to 76 kg of alkali per ton of recycled aggregate.

[0012] By adopting the above technical scheme, the recycled aggregate is obtained by crushing and screening the old concrete. In the production process, the surface of the recycled aggregate has new sections formed by crushing and cracks that penetrate into the original aggregate. There is SiO2 on this surface. When the recycled aggregate is mixed with alkali solution, X+SiO2+OH reaction similar to alkali-aggregate reaction can occur. - →X-Si-Hgel (X is a metal cation) reaction;

[0013] X-Si-Hgel will expand after absorbing water. In the alkali-aggregate reaction, since the aggregate has been prepared into concrete, X-Si-Hgel expands to form a large amount of gel that accumulates and expands at the interface of concrete aggregate, causing uneven expansion and cracking of the concrete along the interface.

[0014] In the present application, it is advantageous to make the recycled aggregate send out a similar reaction before preparation, and the reaction is advantageous to make the X-Si-Hgel located in the cracks repair and fill the cracks, and the X-Si-Hgel located on the surface of the recycled aggregate forms a new surface on the surface of the recycled aggregate - the bonding force between the surface and the cement slurry is due to the original cement slurry;

[0015] This reduces the water absorption of the recycled aggregate and reacts the SiO2 on the newly exposed surface of the recycled aggregate in advance, weakening the alkali-aggregate reaction. On the other hand, it also forms a new surface with strong bonding with cement slurry, making the bonding strength between the modified recycled aggregate and the new cement slurry in the early strength stage much higher than that of ordinary recycled aggregate.

[0016] At the same time, non-calcined shell powder is also added to the concrete raw materials of the present application, and the non-calcined shell powder contains organic matter such as chitin and amino acids. After the concrete raw materials are mixed, the alkalinity in the water environment continues to increase due to the hydration reaction, and due to the modified recycled aggregate of the present application, the alkalinity of the recycled concrete of the present application is stronger than that of the concrete using ordinary recycled aggregate. Although the alkaline substance plays a protective role on the metal components in the concrete body after the concrete solidifies, excessive alkalinity will lead to the strengthening of the alkali-aggregate reaction.

[0017] In this application, the alkali-aggregate reaction of the modified recycled aggregate is weakened after treatment, but the alkaline substances brought in will affect the alkali-aggregate reaction of the natural aggregate. For this reason, non-calcined shell powder is specifically added in this application, and its chitin and amino acids can react with the alkaline substances in the water environment before the concrete solidifies, consume the alkaline substances, and the reaction is more likely to occur with the increase of alkalinity strength, thereby controlling the alkalinity of the water environment before the concrete solidifies, avoiding excessive alkalinity in the water environment, and preventing the cracking and strength reduction of the concrete caused by the excessive alkali-aggregate reaction of the natural aggregate.

[0018] On the other hand, chitosan or similar polymers produced by the reaction of chitin in non-calcined shell powder with alkaline substances have a bonding effect, which can improve the bonding properties of cement mortar in concrete, thereby further improving the early tensile strength of recycled concrete.

[0019] In summary, the recycled concrete of the present application uses the modified recycled aggregate and non-calcined shell powder of the present application at the same time, and the two work synergistically to improve the recycled aggregate, enhance the bonding performance of cement mortar without affecting the natural aggregate, and ultimately improve the early tensile strength of the recycled concrete and reduce the possibility of cracking of the recycled concrete.

[0020] Preferably, the pH value of the alkali solution is 11-12.

[0021] By adopting the above technical scheme, the alkali solution is prepared by alkali, and its pH reflects the concentration of hydroxide ions in the alkali solution. The alkali solution with too low pH has a slow reaction speed and insufficient activation effect. It needs to use more additional alkali solution, and the increased alkaline substances have a greater impact on the alkali-aggregate reaction of natural aggregates, so it is not good. The alkali solution with too high pH has a large alkali solution concentration and too little alkali solution. It is absorbed by the recycled aggregate too quickly, and most of the SiO2 on the new surface of the recycled aggregate is not in contact with the alkali solution, resulting in insufficient activation. It also needs to increase the amount of alkali solution, and the increased alkaline substances have a greater impact on the alkali-aggregate reaction of natural aggregates, so it is not good.

[0022] Preferably, the alkali solution is Ca(OH)2.

[0023] By adopting the above technical solution, Ca(OH)2 can reduce the alkali-aggregate reaction of natural aggregate, reduce the possibility of cracks, and improve the impermeability of the concrete body.

[0024] Optional: the raw materials also include 50 to 65 parts of plant fiber silk.

[0025] By adopting the above technical scheme, adding plant fiber filaments can strengthen the internal cracking resistance of concrete during the initial setting to final setting of concrete, and resist the expansion cracking under the hydration heat; at the same time, the plant fiber filaments can serve as a moisture migration channel in the uncured concrete, the moisture penetration and distribution in the concrete body is more uniform, the hydration reaction in the concrete body is more uniform, and the high-temperature concrete with strong local hydration conducts heat to the surrounding low-temperature concrete more quickly through water, reducing the situation of local hydration heat overheating, and in general reducing the possibility of cracks in the concrete casting body.

[0026] Optionally, the plant fiber filaments are obtained by fermenting and crushing the plant fibers.

[0027] By adopting the above technical scheme, the fermented plant fiber filaments can allow more ions and colloids to penetrate into the plant fiber filaments. During the concrete hydration reaction and curing process, the plant fiber filaments undergo changes similar to mineralization, gradually reducing the gaps and air inside the plant fiber filaments, making the cured concrete denser and improving the concrete's anti-permeability performance.

[0028] Optionally, the plant fiber filaments are fermented by the following method:

[0029] The plant fiber is mixed with another raw material, non-calcined shell powder, and then fermented.

[0030] By adopting the above technical scheme, plant fiber and non-calcined shell powder are fermented together. For plant fiber, non-calcined shell powder has a certain moisture absorption and water storage effect, which is convenient for controlling the water content of plant fiber during fermentation, avoiding excessive fermentation and reduced strength, and insufficient fermentation and subsequent similar mineralization transformation. For non-calcined shell powder, the bacteria and its metabolites in the fermentation liquid produced by plant fiber fermentation can depolymerize the chitin in the non-calcined shell powder, reduce the difficulty of subsequent reaction of non-calcined shell powder with alkaline substances in concrete, and improve the alkali control effect of non-calcined shell powder.

[0031] Optional: The fermentation conditions are relative humidity 58±5%, temperature 28±2°C, and fermentation time 3 to 4 days.

[0032] By adopting the above technical scheme, the raw materials after mixed fermentation of plant fiber silk and non-calcined shell powder under the fermentation conditions are used, which has a better effect on recycled concrete.

[0033] Optionally, the recycled aggregate and the alkali solution are mixed by spraying the alkali solution onto the stirred recycled aggregate.

[0034] By adopting the above technical solution, the mixing method of stirring and spraying alkali solution can make the mixing more uniform, and the SiO2 on the surface of the recycled aggregate can be guaranteed to undergo X+SiO2+OH reaction with less alkali. -→X-Si-Hgel (X is a metal cation) reaction is more comprehensive.

[0035] In summary, the present invention has the following beneficial effects:

[0036] 1. The application for recycled concrete uses the modified recycled aggregate and non-calcined shell powder of this application at the same time. The two work synergistically to improve the recycled aggregate and the bonding performance of cement mortar without affecting the natural aggregate, ultimately improving the early tensile strength of the recycled concrete and reducing the possibility of cracking of the recycled concrete;

[0037] 2. In this application, plant fiber filaments are added to enhance the concrete's resistance to hydration and thermal cracking, and the plant fiber filaments are pre-fermented, which can cause the plant fiber filaments to undergo a mineralization-like reaction during the concrete curing process, thereby ensuring the concrete's impermeability. DETAILED DESCRIPTION

[0038] Source of raw materials:

[0039] The non-calcined shell powder is obtained by crushing and sieving the shells, and has a particle size of 0.2 to 0.4 mm.

[0040] The cement is commercially available 42.5 silicate.

[0041] The particle size of recycled aggregate is 4 to 5 cm.

[0042] The particle size of natural aggregate is 7 to 10 cm.

[0043] The sand is 0.3~0.6mm.

[0044] The plant fiber is wheat straw or rice stalk.

[0045] Example 1

[0046] A recycled concrete comprising the following raw materials in parts by weight:

[0047] Natural aggregate 2000kg,

[0048] Modified recycled aggregate 8000kg,

[0049] Cement 4200kg;

[0050] Sand 400kg;

[0051] Uncalcined shell powder 1560kg;

[0052] 3300kg of water.

[0053] The modified recycled aggregate is obtained by activation modification of recycled aggregate, and the activation modification method is as follows:

[0054] Add alkali solution to the recycled aggregate while stirring it, continue stirring for 30 minutes after spraying, and then let it stand.

[0055] During the standing period, water is sprayed according to the air humidity to keep the surface of the recycled aggregate not dry and without free water flow. The standing time is 5 hours, and then it is left to dry naturally to obtain modified recycled aggregate.

[0056] The alkali solution is prepared by calcium hydroxide, and its pH is 12. The amount of alkali solution is recorded as alkali amount, which is 50kg alkali per ton of recycled aggregate.

[0057] The preparation method of recycled concrete is as follows:

[0058] The non-calcined shells, natural aggregates, modified recycled aggregates, sand and water are mixed and stirred uniformly to obtain recycled concrete.

[0059] Embodiments 2 to 9

[0060] A recycled concrete is similar to Example 1, except that the amount of raw materials used and the reagent parameters in the activation and modification process of the modified recycled aggregate are different. The specific differences are shown in Table 1 below.

[0061] Table 1. Raw material dosage and modified recycled aggregate modification parameters of Examples 1 to 9

[0062]

[0063] Example 10

[0064] A recycled concrete is similar to Example 1, except that the activation modification method of the modified recycled aggregate is different. The activation modification of the modified recycled aggregate in Example 10 is as follows:

[0065] Add recycled aggregate to the alkali solution, stir and mix for 1 hour and then let it stand. During the standing period, spray water according to the air humidity to keep the surface of the recycled aggregate not dry and without free water flow. The standing time is 5 hours, and then wait for natural drying to obtain modified recycled aggregate.

[0066] The alkali solution is made of calcium hydroxide and has a pH of 12. The ratio of alkali solution to recycled aggregate is 50 kg alkali to 1 ton of recycled aggregate.

[0067] Comparative Example 1

[0068] A recycled concrete is similar to Example 1, except that no non-calcined shell powder is added to the raw materials, that is, the amount of non-calcined shell powder is 0.

[0069] Comparative Example 2

[0070] A recycled concrete is similar to Example 1, except that the modified recycled aggregate is replaced with an equal mass of non-activated modified recycled aggregate.

[0071] Comparative Example 3

[0072] A recycled concrete is similar to Example 1, except that the amount of non-calcined shell powder is 0, and the quality of non-activated modified recycled aggregate is used to replace the modified recycled aggregate.

[0073] The recycled concrete obtained in Examples 1 to 9 and the recycled concrete obtained in Comparative Examples 1 to 3 were subjected to crack observation experiments, early tensile strength tests, and anti-permeability tests.

[0074] Crack observation experiment: A test was conducted to determine whether cracks in large-volume recycled concrete bodies would affect their appearance during the solidification process. The recycled concrete was poured into a 1.8m*1.8m*0.4m mold and vibrated to obtain a sample. After 7 days of curing, the sample was tested for cracks on the surface. No cracks were recorded as 1, 1 to 3 cracks with a crack width not exceeding 0.5mm were recorded as 2, 4 to 6 cracks with a crack width not exceeding 0.5mm were recorded as 3, and more than 6 cracks or crack widths greater than 0.5mm were recorded as 4.

[0075] The early tensile strength test is to test the tensile strength of recycled concrete on the 7th day after pouring according to the axial tensile strength test in GB / T 50081-2019.

[0076] The impermeability test is based on GB / T 50082-2009 to test the impermeability of recycled concrete on the 28th day after pouring, expressed in terms of impermeability grade.

[0077] The test results are shown in Table 2 below.

[0078] Table 2. Crack observation, early tensile strength and impermeability test results of Examples 1 to 9 and Comparative Examples 1 to 3

[0079]

[0080]

[0081] Combined with Table 2, by comparing Examples 1 to 3 with Comparative Examples 1 to 3, it can be seen that the early tensile strength of the recycled concrete Examples 1 to 3 of the present application is much greater than that of the ordinary recycled concrete of Comparative Example 3, and the recycled concrete of the present application has good crack resistance to the heat of concrete hydration. In terms of actual surface appearance, the recycled concrete of the present application is better than the ordinary recycled concrete of Comparative Example 3. At the same time, after 28 days, the recycled concrete of the present application also exhibits better anti-permeability performance than the ordinary recycled concrete of Comparative Example 3.

[0082] Therefore, the recycled concrete of the present application has better resistance to cracking caused by hydration heat in the early stage of concrete curing than the existing ordinary recycled concrete, and has good anti-permeability after complete curing.

[0083] By comparing Example 2 and Comparative Example 2, it can be seen that in Comparative Example 1, non-calcined shell powder was added but the recycled aggregate was not modified. Its appearance was severely cracked and its early tensile strength was significantly lower than that of Example 2. This was due to the large amount of absorption by the recycled aggregate and the poor bonding with the new cement mortar. The addition of non-calcined shell powder alone could not reduce the water absorption of the recycled aggregate or improve the bonding between the recycled aggregate and the new cement mortar.

[0084] At the same time, it can be seen from Comparative Examples 1 and 3 that when only the recycled aggregate is modified in Comparative Example 1, its early tensile strength and impermeability after curing are far inferior to those of ordinary recycled concrete. The reason is that in the modification process, the cracks of the recycled aggregate must be sealed and a new bonding surface with strong bonding strength must be formed on the surface. The concentration of the alkali solution used must be high to promote the reaction. At the same time, the high water absorption of recycled concrete requires a large amount of alkali solution. The actual amount of alkali used exceeds the amount required for the modification of the recycled aggregate. The residual alkali aggravates the original inevitable alkali-aggregate reaction of the natural aggregate, resulting in the recycled concrete being more prone to cracking, more internal cracks, and worse impermeability.

[0085] In this application, non-calcined shell powder and modified recycled aggregate are used at the same time. Compared with calcined shell powder, non-calcined shell powder contains chitin and amino acids. After being mixed with concrete raw materials, the non-calcined shell powder can react with the excess alkali brought in during the modification process and the alkali generated by the hydration reaction, neutralize the alkalinity and inhibit the alkali-aggregate reaction of natural aggregate.

[0086] The alkali reaction of non-calcined shell powder is more likely to occur as the alkalinity increases, and is not easy to occur when the alkalinity is low. This matches the mechanism of continuously producing new alkaline substances during the hydration process of concrete. Therefore, the non-calcined shell powder only neutralizes excess alkaline substances, and there is no need to neutralize all alkaline substances in the recycled concrete. In the case of a small amount, a good control mechanism for the alkaline strength of the recycled concrete can be formed - the reaction is not easy to occur in a low-alkaline environment, and retaining a certain alkalinity of the concrete body is beneficial to protect the metal parts in the concrete body. The reaction is easy to occur in a high-alkaline environment, consuming too much alkali and reducing the alkalinity.

[0087] In addition, chitosan or similar derivatives that are depolymerized by the chitin in the non-calcined shell powder under alkaline conditions have a bonding effect, which can strengthen the bonding properties of cement mortar, improve the bonding properties between cement mortar and natural aggregate, and between cement mortar and recycled aggregate, thereby improving the recycled concrete's resistance to hydration thermal cracking and impermeability.

[0088] By comparing Example 2 with Example 4 and Example 5, it can be seen that the alkali solution in the present application can also be configured with NaOH or KOH. Among the three, Ca(OH)2 is selected to configure the alkali solution to modify the recycled aggregate, which has better performance for the final product, recycled concrete.

[0089] Compared with Examples 6 to 13, the amount of alkali in the alkali solution used in Examples 6 to 13 remains unchanged. When the concentration of the alkali solution is continuously increased, it can be seen from the experimental results that as the concentration of the alkali solution increases, the crack observation results of the recycled concrete show that the cracks first decrease and then increase with the increase of the concentration, the early tensile strength first increases and then decreases, and the impermeability grade first increases and then decreases;

[0090] This is because the activation and modification effect of recycled aggregates is poor due to low alkali solution concentration. As the concentration increases, the activation and modification effect of recycled aggregates increases, which can improve the performance of recycled concrete.

[0091] However, as the concentration of alkali solution increases, the amount of alkali solution will decrease under the same alkali dosage, and it will be absorbed by the recycled aggregate too quickly. Most of the SiO2 on the new surface of the recycled aggregate will not come into contact with the alkali solution, resulting in insufficient activation modification and reduced performance improvement of the recycled concrete.

[0092] Increasing the amount of alkali solution under high concentration alkali solution will make the alkali amount exceed the control buffer range of non-calcined shell powder, and increase the impact on the alkali-aggregate reaction of natural aggregate. As in Example 1, the residual alkali aggravates the original inevitable alkali-aggregate reaction of natural aggregate, resulting in the recycled concrete being more prone to cracking, having more internal cracks, and having worse impermeability. In summary, the alkali solution pH of this application is preferably selected to be 11-12.

[0093] Comparing Example 2 and Example 10, compared with Example 1, the alkali solution in Example 10 is not in sufficient contact with the surface of the recycled aggregate, and is absorbed into the interior of the recycled aggregate too quickly, resulting in insufficient activation modification and reduced performance improvement of the recycled concrete. In the present application, it is better to use the alkali solution mixing method while stirring the recycled aggregate and spraying the alkali solution.

[0094] Embodiment 11

[0095] A recycled concrete comprising the following raw materials in parts by weight:

[0096] Natural aggregate 3500kg,

[0097] Modified recycled aggregate 6500kg,

[0098] 4000kg cement;

[0099] Sand 4800kg;

[0100] 1410kg of non-calcined shell powder;

[0101] Plant fiber 500kg

[0102] 3300kg of water.

[0103] The modified recycled aggregate is the same as the modified recycled aggregate used in Example 1 and is from the same batch.

[0104] The plant fiber is rice stalks or wheat straws, in this case rice stalks.

[0105] Plant fibers are first pretreated:

[0106] The plant fiber is cut into plant fiber filaments with a length of 3 to 5 cm and a width of 1 to 2 mm. The plant fiber filaments are mixed with another raw material, non-calcined shell powder, and fermented for 3 to 4 days by using the plant fiber's own bacteria under conditions of relative air humidity of 58±5% and temperature of 23±2°C to obtain pretreated materials.

[0107] The preparation method of recycled concrete is as follows:

[0108] The pre-treated material, natural aggregate, modified recycled aggregate, sand and water are mixed and stirred evenly to obtain recycled concrete.

[0109] Example 12

[0110] A recycled concrete, similar to Example 11, except that the amount of plant fiber used is 600 kg.

[0111] Embodiment 13

[0112] A recycled concrete, similar to Example 11, except that the amount of plant fiber used is 650 kg.

[0113] Examples 14 to 26

[0114] A recycled concrete is similar to Example 12, except that the parameters of the pretreatment method of the plant fiber are different. The specific differences are shown in Table 3 below.

[0115] Table 3. Parameters of plant fiber pretreatment method of Example 12 and Examples 14 to 26

[0116] Fermentation relative humidity / % Fermentation temperature / ℃ Fermentation time / day Example 12 58±5 28±2 3.6 Embodiment 14 58±5 28±2 3 Embodiment 15 58±5 28±2 4 Example 16 48±5 28±2 3 Embodiment 17 48±5 28±2 3.6 Embodiment 18 48±5 28±2 4 Embodiment 19 68±5 28±2 3 Embodiment 20 68±5 28±2 3.6 Embodiment 21 68±5 28±2 4 Embodiment 22 58±5 33±2 3 Embodiment 23 58±5 33±3 3.6 Embodiment 24 58±5 33±4 4 Embodiment 25 58±5 23±2 3 Embodiment 26 58±5 23±2 4

[0117] Embodiment 27

[0118] A recycled concrete, which differs from Example 12 in that the plant fiber pretreatment method is as follows: the plant fibers are cut into plant fiber filaments with a length of 3 to 5 cm and a width of 1 to 2 mm, and the plant fiber filaments and non-calcined shell powder are directly mixed with other raw materials to prepare recycled concrete.

[0119] Embodiment 28

[0120] A recycled concrete, which differs from Example 12 in the pretreatment method of plant fibers, is as follows:

[0121] The plant fiber is cut into plant fiber strands with a length of 3 to 5 cm and a width of 1 to 2 mm. The plant fiber strands are fermented for 3 to 4 days under the conditions of relative air humidity of 58±5% and temperature of 23±2°C by using the plant fiber's own bacteria to obtain pretreated materials.

[0122] Embodiment 29

[0123] A recycled concrete comprising the following raw materials in parts by weight:

[0124] Natural aggregate 3000kg,

[0125] Modified recycled aggregate 7000kg,

[0126] Cement 4200kg;

[0127] Sand 4000kg;

[0128] Uncalcined shell powder 1560kg;

[0129] Plant fiber 625kg

[0130] 3300kg of water.

[0131] The modified recycled aggregate is the same as the modified recycled aggregate used in Example 1 and is from the same batch.

[0132] The plant fiber is rice stalks or wheat straws, in this case rice stalks.

[0133] Plant fibers are first pretreated:

[0134] The plant fiber is cut into plant fiber filaments with a length of 3 to 5 cm and a width of 1 to 2 mm. The plant fiber filaments are mixed with another raw material, non-calcined shell powder, and fermented for 3 to 4 days by using the plant fiber's own bacteria under conditions of relative air humidity of 58±5% and temperature of 23±2°C to obtain pretreated materials.

[0135] The preparation method of recycled concrete is as follows:

[0136] The pre-treated material, natural aggregate, modified recycled aggregate, sand and water are mixed and stirred evenly to obtain recycled concrete.

[0137] Embodiment 30

[0138] A recycled concrete comprising the following raw materials in parts by weight:

[0139] Natural aggregate 4000kg,

[0140] Modified recycled aggregate 6000kg,

[0141] Cement 3500kg;

[0142] Sand 4500kg;

[0143] 1200kg of non-calcined shell powder;

[0144] Plant fiber 550kg

[0145] 3300kg of water.

[0146] The modified recycled aggregate is the same as the modified recycled aggregate used in Example 1 and is from the same batch.

[0147] The plant fiber is rice stalks or wheat straw, in this case wheat straw.

[0148] Plant fibers are first pretreated:

[0149] The plant fiber is cut into plant fiber filaments with a length of 3 to 5 cm and a width of 1 to 2 mm. The plant fiber filaments are mixed with another raw material, non-calcined shell powder, and fermented for 3 to 4 days by using the plant fiber's own bacteria under conditions of relative air humidity of 58±5% and temperature of 23±2°C to obtain pretreated materials.

[0150] The preparation method of recycled concrete is as follows:

[0151] The pre-treated material, natural aggregate, modified recycled aggregate, sand and water are mixed and stirred evenly to obtain recycled concrete.

[0152] The recycled concrete obtained in Examples 11 to 30 was tested, wherein the mold size used for crack observation was changed to 1.8m*1.8m*0.8m. Similarly, a crack observation experiment with a mold size of 1.8m*1.8m*0.8m was performed on Example 2, and the test structure is shown in Table 4 below.

[0153] Table 4. Crack observation, early tensile strength and impermeability test results of Example 2 and Examples 11 to 30

[0154]

[0155]

[0156] This application makes further research based on the more serious cracking caused by uneven hydration heat when recycled concrete is used in larger concrete volumes (thickness greater than 0.5m).

[0157] From Table 4, it can be seen from the comparison between Example 2 and Example 27 that the addition of plant fiber filaments to the recycled concrete raw materials of the present application can improve the early tensile strength of the recycled concrete and improve the anti-cracking performance; on the other hand, the plant fiber filaments migrate and redistribute the moisture in the recycled concrete, regulate the hydration heat distribution in the concrete, and reduce the occurrence of cracks.

[0158] By comparing Example 27 and Example 28, it can be seen that the plant fiber filaments are first fermented, and the ions and silicate colloid produced during the concrete hydration process can more easily penetrate into the plant fiber filaments, occupy the gaps in the plant fibers, and produce a mineralization-like reaction on the plant fibers, so that the recycled concrete is more dense during the curing process, and the water permeability of the plant fibers infiltrated by silicate colloid after curing is reduced, thereby improving the anti-seepage performance of the recycled concrete.

[0159] By comparing Examples 11 to 13 and Example 28, it can be seen that in Examples 11 to 13, the non-calcined shell powder and the plant fiber silk are fermented together, and the obtained pretreated material and other raw materials are used to prepare recycled concrete, and the obtained concrete early tensile strength and impermeability strength are better than those in Example 28. The reason is that the plant fiber and the non-calcined shell powder are fermented together. For the plant fiber, the non-calcined shell powder has a certain moisture absorption and water storage effect, which is convenient for controlling the water content of the plant fiber during the fermentation process, avoiding excessive fermentation and strength reduction, and insufficient fermentation and subsequent similar mineralization transformation; for the non-calcined shell powder, the bacteria and its metabolites in the fermentation liquid produced by the fermentation of the plant fiber can have a pre-depolymerization effect on the chitin in the non-calcined shell powder, reducing the difficulty of the subsequent non-calcined shell powder to react with alkaline substances in concrete, and improving the alkali control effect of the non-calcined shell powder and the bonding enhancement effect of the reactants.

[0160] By comparing Example 2 with Examples 14 to 26, it can be seen that the fermentation time, relative humidity of the air during fermentation and fermentation temperature during the fermentation of plant fiber and non-calcined shell powder all affect the performance of recycled concrete using pretreated materials.

[0161] The fermentation time, relative humidity of the air during fermentation, and fermentation temperature are interrelated to affect the degree of fermentation:

[0162] Short fermentation time, low fermentation humidity and low fermentation temperature are not conducive to fermentation. Insufficient fermentation will lead to insufficient fermentation of plant fiber filaments and insufficient pre-depolymerization of non-calcined shell powder, insufficient subsequent mineralization transformation of plant fiber filaments, and weakening of the alkali control and viscosity increasing effects of non-calcined shell powder, resulting in reduced improvement in anti-permeability performance.

[0163] High fermentation temperature can promote fermentation in a short time, but long fermentation will lead to over-fermentation. Fermentation time is too long and humidity is high, which may lead to over-fermentation. Over-fermentation will reduce the strength of plant fiber and lead to a decrease in the early tensile strength of recycled concrete.

[0164] The fermentation conditions in this application are relative humidity 58±5%, temperature 28±2°C, and the fermentation time is preferably 3 to 4 days.

[0165] It can be seen from Examples 29 and 30 that wheat straw can also be used as plant fiber in the present application, and the recycled concrete of the present application has universal applicability when applied to large-volume concrete bodies.

[0166] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A recycled concrete that resists hydration thermal cracking, It is characterized in that Including the following raw materials by mass: 200~400 parts of natural aggregate; 600~800 parts of modified recycled aggregate; 350~420 parts of cement; Sand 400~480 parts; 120-156 parts of non-calcined shell powder; 50~65 parts of plant fiber; The modified recycled aggregate is obtained by activating the recycled aggregate mixed with alkali solution, wherein the alkali solution is Ca(OH) 2 The pH of the alkali solution is 11-12, and the amount of the alkali solution is 50-76 kg per ton of recycled aggregate. The plant fiber filaments are obtained by shearing the plant fibers; The plant fiber strands are mixed with non-calcined shell powder and fermented; The fermentation conditions are relative humidity 58±5%, temperature 28±2°C, and fermentation time 3-4 days.

2. The recycled concrete resistant to hydration thermal cracking according to claim 1, It is characterized in that The method for mixing the recycled aggregate and the alkali solution is to spray the alkali solution onto the stirred recycled aggregate.