Waterborne polyurethane coating for elastic base surface protection and preparation method thereof

By developing water-based polyurethane coatings for plastic floors, we solve the problem of frequent waxing and maintenance of plastic floors, provide environmental protection and weather resistance, meet daily disinfection needs, reduce operating costs and reduce environmental pollution.

CN116496687BActive Publication Date: 2024-10-18全毅
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310520542.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-10-18
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

Plastic floors require frequent waxing and maintenance, which leads to problems such as not being wear-resistant, unable to meet daily disinfection, high cost, environmental pollution, not environmentally friendly, and not low-carbon.

Method used

Develop a water-based polyurethane coating for surface protection of elastic base layers, including a first water-based acrylic resin, a second water-based acrylic resin, a polyether siloxane copolymer, a water-based silane accelerator and a silane compound containing an epoxy group, by Specific formulations and preparation methods create weather- and abrasion-resistant coatings.

Benefits of technology

This coating provides environmental protection, weather resistance and wear resistance, can replace traditional waxing and maintenance, meet daily disinfection needs, reduce operating costs, reduce environmental pollution, and is easy to construct.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116496687B_ABST
    Figure CN116496687B_ABST
Patent Text Reader

Abstract

The present invention relates to a water-based polyurethane coating for elastic base surface protection, comprising a mixed component A and a component B, wherein the component A comprises a first water-based acrylic resin, a second water-based acrylic resin, a polyether siloxane copolymer, a water-based silane accelerator, a silane compound containing an epoxy group and a coating auxiliary material; and the component B is a curing agent. The coating of the present invention is an environmentally friendly material, and the coating formed by the coating has excellent water resistance, acid and alkali resistance, a smooth and dense surface, so that stains are easy to wipe off, and has excellent aging resistance, which can ensure that it does not fade after long-term use and does not affect the appearance. The coating has a low cost and is easy to construct, which can create convenient conditions for large-scale promotion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic floor protection, in particular to a waterborne polyurethane coating for elastic base surface protection and a preparation method thereof. Background Art

[0002] Plastic floor is a new type of lightweight floor decoration material that is very popular in the world today, also known as "lightweight floor material". Plastic floor is made of polyvinyl chloride as raw material, with fillers, plastic steel materials, powder, stabilizers and other auxiliary materials added, and is produced through extrusion, lamination and coating processes. It has been widely recognized in large and medium-sized cities in China and is widely used in various systems.

[0003] Advantages of plastic flooring: green and environmentally friendly, ultra-light and ultra-thin, excellent anti-slip properties, sound absorption and noise reduction, antibacterial, and a wide variety of patterns and colors.

[0004] The disadvantage of plastic floor is that it needs to be waxed and maintained regularly. Usually, composite plastic floor is waxed and maintained 4 times a year, and homogeneous plastic floor is generally waxed and maintained once a month. Only in this way can the service life of plastic floor be extended and the practicality of plastic floor be ensured. Frequent waxing has many problems, such as:

[0005] 1. Not wear-resistant. In corridors and doorways with heavy traffic, the wax is worn off before the normal maintenance period, and the plastic floor cannot be protected. Part of the plastic floor is often worn out with obvious scratches and stains. These scratches and stains cannot be removed by simple cleaning.

[0006] 2. It cannot meet the daily disinfection needs. In hospitals, 84 disinfectant is usually used for daily disinfection. Its main component is sodium hypochlorite, which has strong corrosive and bleaching properties and will cause irreversible corrosion and discoloration to plastic floors.

[0007] 3. High cost. One waxing maintenance costs about 10 yuan, 4 times a year, and the annual maintenance cost is 40 yuan. The maintenance cost of 3 years can be used to make a new layer of plastic floor.

[0008] 4. Long interruption cycle for users. Each time waxing and maintenance is performed, the base layer needs to be ground, cleaned, waxed, and maintained. The basic cycle is about 2-5 days. Each maintenance requires users to suspend business to cooperate.

[0009] 5. Not environmentally friendly. Every time the base layer is dewaxed and cleaned during maintenance, a large amount of wastewater and waste will be generated. Wastewater is generally discharged directly into the pipe network, polluting water resources. Waste is polluted along with domestic garbage, polluting the environment.

[0010] 6. Not low-carbon. Regular maintenance not only produces a large amount of wastewater and has an impact on the environment, but also consumes manpower, financial resources, and material resources, which is inconsistent with the low-carbon and environmental protection strategy advocated by the country.

[0011] In view of these situations of plastic floor, there is an urgent need for a coating that can be applied to the surface of the plastic floor to replace traditional waxing maintenance. Summary of the invention

[0012] The purpose of the present invention is to provide a water-based polyurethane coating for protecting the surface of an elastic base layer, which replaces the traditional waxing and maintenance of plastic floors and has environmental protection and excellent weather resistance and wear resistance.

[0013] To achieve the above object, the present invention adopts the following technical solutions:

[0014] A waterborne polyurethane coating for elastic base surface protection, comprising a mixed component A and a component B, wherein:

[0015] The component A comprises a first water-based acrylic resin, a second water-based acrylic resin, a polyether siloxane copolymer, a water-based silane accelerator, a silane compound containing an epoxy group and coating auxiliary materials;

[0016] The component B is a curing agent.

[0017] The water-based polyurethane coating for elastic base surface protection, preferably, the addition amount of the polyether siloxane copolymer is not less than 2% of the total weight of the component A, the addition amount of the water-based silane accelerator is not less than 2.5% of the total weight of the component A, and the addition amount of the epoxy-containing silane compound is not less than 2% of the total weight of the component A.

[0018] The water-based polyurethane coating for elastic base surface protection, preferably, the addition amount of the polyether siloxane copolymer is 2%-5% of the total weight of the component A, the addition amount of the water-based silane accelerator is 2.5%-5% of the total weight of the component A, and the addition amount of the epoxy-containing silane compound is 2%-5% of the total weight of the component A.

[0019] The water-based polyurethane coating for elastic base surface protection is preferably such that the first water-based acrylic resin is a water-based hydroxyl-functional polyacrylate dispersion, the second water-based acrylic resin is an anionic polyacrylate dispersion, the first water-based acrylic resin is added in an amount of 35-40% of the total weight of component A, and the second water-based acrylic resin is added in an amount of 35-40% of the total weight of component A.

[0020] The water-based polyurethane coating for elastic base surface protection, preferably, the first water-based acrylic resin is a water-based hydroxyl-functional polyacrylate dispersion, the second water-based acrylic resin is an anionic polyacrylate dispersion, the addition amount of the first water-based acrylic resin is 35% of the total weight of the component A, and the addition amount of the second water-based acrylic resin is 35% of the total weight of the component A.

[0021] The waterborne polyurethane coating for elastic base surface protection, preferably, the coating auxiliary materials include a wetting agent, a defoamer, a thickener and deionized water, and the added amount of each component of the coating auxiliary materials accounts for the percentage of the total weight of the component A:

[0022]

[0023] The waterborne polyurethane coating for elastic base surface protection, preferably, the added amount of each component of the coating auxiliary material accounts for the percentage of the total weight of the component A:

[0024]

[0025] The water-based polyurethane coating for elastic base surface protection, preferably, the thickener includes water-based non-ionic associative polyurethane and solvent-free non-ionic associative polyurethane, the addition amount of the water-based non-ionic associative polyurethane accounts for 1% of the total weight of the component A, and the addition amount of the solvent-free non-ionic associative polyurethane accounts for 1% of the total weight of the component A.

[0026] In the waterborne polyurethane coating for elastic base surface protection, preferably, the curing agent is a hydrophilic aliphatic polyisocyanate of hexamethylene diisocyanate.

[0027] A method for preparing component A in a waterborne polyurethane coating for elastic base surface protection, the specific steps are as follows:

[0028] Add the formula deionized water, the first water-based acrylic resin and the second water-based acrylic resin, disperse at a speed of 600 r / min for 5 minutes;

[0029] Add wetting agent and defoamer, speed 1200r / min, disperse for 15 minutes;

[0030] Add thickener, polyether siloxane copolymer, water-based silane accelerator and epoxy-containing silane compound at a speed of 1200 r / min and disperse for 30 minutes;

[0031] Among them, the addition amount of the polyether siloxane copolymer is not less than 2% of the total weight of the component A, the addition amount of the water-based silane accelerator is not less than 2.5% of the total weight of the component A, and the addition amount of the epoxy-containing silane compound is not less than 2% of the total weight of the component A.

[0032] The present invention adopts the above technical solution, which has the following advantages:

[0033] 1. Select water-based acrylic resin and isocyanate curing agent. Mix the two to form water-based polyurethane. Select excellent two-component water-based polyurethane as the basic film-forming substance to lay the foundation for long-term use without discoloration.

[0034] 2. Screen a large number of different types of water-based acrylic emulsions and mix them to produce highly wear-resistant materials with excellent wear resistance.

[0035] 3. To meet the daily disinfection requirements of 84 disinfectant, the material's resistance to disinfection is improved by adding polyether siloxane copolymer.

[0036] 4. Add water-based silane accelerator to improve the bonding strength between the coating and the plastic floor base, and double the protection to solve the problem of interlayer bonding.

[0037] 5. Add silane compounds containing epoxy groups as coupling agents to enhance the cross-linking density of the coating and achieve the effect of anti-penetration.

[0038] 6. The two water-based acrylic resins have different properties: one is to make the paint film have better mechanical resistance, weather resistance and toughness after completion, and the other is to make the paint film have high gloss and acid, alkali and other chemical resistance after completion.

[0039] The coating of the present invention is an environmentally friendly material. The coating formed by the coating has excellent water resistance, acid and alkali resistance, a smooth and dense surface, which makes it easy to wipe off stains, and has excellent aging resistance, which can ensure that it will not fade after long-term use and will not affect the appearance. The coating has a low cost and is easy to construct, which can create convenient conditions for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The wear-resistant effect of different resin contents in component A;

[0041] Figure 2 The effect of adding different contents of A1 on the resistance to 84 disinfectant;

[0042] Figure 3 The effect of adhesion test with different contents of A2 added;

[0043] Figure 4 The effect of adding different contents of A3 on the iodine resistance test;

[0044] Figure 5 To test the adhesion and iodine resistance of adding different contents of A2 and A3. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0046] The present invention takes plastic floor as the object, and conducts film-forming material and coupling agent

[0047] 1. Selection of basic film-forming materials

[0048] 1. Numerical performance comparison

[0049] Commonly used water-based resins include water-based acrylic resins, water-based epoxy resins and water-based polyurethane resins. Water-based acrylic resins, water-based epoxy resins and water-based polyurethane resins are mass products. Performance comparison tests were conducted on water-based acrylic resins, water-based epoxy materials and water-based polyurethane materials to select the best basic film-forming substances. The test data is shown in Table 1:

[0050] Table 1 Comparative test of resin performance

[0051]

[0052]

[0053] Test data show that the coating with waterborne polyurethane as the basic film-forming material has much better bonding strength with the substrate, water resistance, acid and alkali resistance, and aging resistance than waterborne acrylic resin and waterborne epoxy coatings. Based on current test results, waterborne polyurethane material is the most ideal basic film-forming material.

[0054] 2. Coating density test

[0055] The coating density of coatings based on water-based acrylic, water-based epoxy and water-based polyurethane film-forming substances was tested to compare which one is the best. The results are shown in Table 2.

[0056] Table 2 Coating density test

[0057]

[0058] According to the standard JC / T908-2013, the stain resistance value ranges from 1 to 5. The smaller the value, the better the stain resistance performance. The stain resistance index is the sum of the stain resistance values ​​tested by all reagents. The test data shows that water-based epoxy has poor organic acid resistance, and water-based acrylic is not resistant to solution penetration. Stain resistance index: water-based polyurethane < water-based epoxy < water-based acrylic, stain resistance performance: water-based polyurethane > water-based epoxy > water-based acrylic.

[0059] The test data show that: from the sum of the stain resistance values, it can be clearly seen that the water-based polyurethane coating has better anti-fouling performance than water-based acrylic and water-based epoxy coatings.

[0060] Based on the above test results, water-based polyurethane was selected as the base material for the plastic floor protective agent coating.

[0061] 2. Research on finished product formula

[0062] 1. Test the wear resistance of different resin contents

[0063] The specific ingredients of each component formula are shown in Table 3 and Table 4:

[0064] Table 3 Ingredients of Component A

[0065]

[0066] Table 4 Ingredients of component B

[0067]

[0068] Wear resistance test method: Apply the material on a special glass plate, fix it on an abrasion tester, add a weight of 750g, rub the coating with a rubber grinding wheel for 500 revolutions, then remove the remaining grinding chips with lint-free paper, and use an analytical balance to record the mass difference before and after grinding, accurate to 0.001g. Test three groups and take the average value.

[0069] GB / T 22374-2018 Floor Coating Materials stipulates that the wear resistance of water-based floor coating materials (type S) (750g / 500r) / g≤0.050g is considered qualified. Figure 1 As shown, all 9 test groups meet the requirements of national standards. Among them, the wear resistance data of groups 5, 6, 8, and 9 are all less than 0.010g, which is even better.

[0070] Through the auxiliary test of wear resistance, we can draw the following conclusions: Test groups 5, 6, 8, and 9 meet the best performance, that is, the addition amount of the first water-based acrylic resin is between 35% and 40%, and the addition amount of the second water-based acrylic resin is between 35% and 40%. Combined with the material cost price, test group 5 was finally selected as the final product formula, in which the addition amount of the first water-based acrylic resin was 35%, and the addition amount of the second water-based acrylic resin was 35%.

[0071] According to the test of a third-party testing agency, the wear resistance index is 0.008g. The wear resistance index is converted into the pressure in actual application, which is convenient for calculating the service life of the material.

[0072] The conversion method is as follows: The weight of the grinding wheel used for testing is 750g and the contact area is 1cm 2 , its pressure on the base is 7.35*10 4 Pa. Assuming that the human body weighs 80 kg, the area of ​​the two feet is 10cm*30cm*2, the pressure of the human body on the base is 1.31*10 4 Pa. The pressure of the test grinding wheel on the base layer is 5.6 times that of the human body on the base layer. The weight of the material of the present invention applied on the surface of the plastic floor is 120g. The grinding wheel rotates 500 times, and the wear is 0.008g. The grinding wheel needs to rotate 7,500,000 times to completely wear off the coating of the material of the present invention, and the human body needs to rotate 42,000,000 times to completely wear off the coating of the material of the present invention. If the service life of the coating of the present invention is required to be 5 years, then the coating can withstand 8,400,000 cycles of wear per year, and the coating can withstand 23,013 cycles of wear per day. If each person wears one cycle every morning, noon and evening, the coating of the present invention can withstand the wear of 7,671 people. With a frequency of 7,500 people per day and 3 cycles of wear, the material of the present invention can withstand 5 years of wear.

[0073] 2. For 84 disinfectant, screen and determine the corresponding A1 surfactant

[0074] The specific ingredients of each component formula are shown in Table 5 and Table 6:

[0075] Table 5 Composition of component A after adding A1

[0076]

[0077]

[0078] Table 6 Ingredients of component B

[0079]

[0080] Specific test method: According to the national standard GB / T 9266-2009 coating washability test, spray with organic disinfectant solvents commonly used in hospitals, then wipe and test, repeat the operation to see how many times the paint film can withstand damage or color changes.

[0081] Assuming that the hospital performs disinfection three times a day, morning, noon and evening, a total of 1095 times a year, if the scrub resistance of the material can meet 10,000 scrubbing times, then the material of the present invention can be used on the surface of the plastic floor for 9 years without worry. For the user, it improves the performance and greatly reduces the operating cost. Therefore, the standard for passing the test is to withstand 10,000 scrubbing times.

[0082] like Figure 2 As shown, A1 surfactant has obvious resistance to 84 disinfectant. With the increase of added amount, the performance improves rapidly. When the added amount reaches 2%, the performance tends to be stable and can reach 10,000 times.

[0083] That is, when the addition amount of A1 surfactant is 2%, the performance of resisting 84 disinfectant can be met.

[0084] 3. Screen the corresponding A2 coupling agent and measure the interlayer bonding strength

[0085] The specific ingredients of each component formula are shown in Table 7 and Table 8:

[0086] Table 7 Composition of component A after adding A2

[0087]

[0088]

[0089] Table 8 Ingredients of component B

[0090]

[0091] like Figure 3 The test method shown is: temperature 23℃±2℃, humidity less than 55%, paint the material on the glass plate, dry for 168 hours, soak in boiling water for 24 hours, wipe the surface of the paint film with paper, and observe the integrity of the paint film. The higher the integrity, the better the adhesion.

[0092] A2 coupling agent has a relatively obvious effect on improving the adhesion between the coating and the glass plate. As the amount added increases, the performance improves rapidly. When the addition amount reaches 3%, the performance tends to be stable and the paint film integrity rate reaches more than 95%.

[0093] That is, when the addition amount of A2 coupling agent is 3%, the adhesion requirement can be met.

[0094] 4. According to the density of the paint film, select the corresponding A3 coupling agent and measure it

[0095] The specific ingredients of each component formula are shown in Table 9 and Table 10:

[0096] Table 9 Composition of component A after adding A3

[0097]

[0098] Table 10 Ingredients of component B

[0099]

[0100] Specific test method: Temperature 23℃±2℃, humidity less than 55%, paint the material on white or blue plastic floor, dry for 168 hours, drop 3 drops of iodine on the surface of the paint film, and then cover it with a watch glass to prevent volatilization. After 24 hours (clean daily, up to 24 hours), remove the watch glass, wipe off the iodine with a wet paper towel, and check whether the paint film has traces of yellowing caused by iodine penetration.

[0101] like Figure 4 As shown, coupling agent A3 has a relatively obvious increasing effect on improving the iodine resistance of the coating. With the increase of the added amount, the performance improves rapidly. When the added amount reaches 2%, the performance tends to be stable and the iodine resistance meets the requirements of 24 hours.

[0102] That is, when the addition amount of A3 coupling agent is 2%, it can be iodine-resistant and meet the requirements of the hospital.

[0103] 5. Determination of the combined effects of various coupling agents and selection of the optimal combination

[0104] The specific ingredients of each component formula are shown in Table 11 and Table 12:

[0105] Table 11 Composition of component A after adding A1, A2 and A3

[0106]

[0107] Table 12 Ingredients of component B

[0108]

[0109] like Figure 5As shown, the test data show that: the combined use of A2 and A3 coupling agents does not have a mutually reducing effect, and A3 coupling agent has a supplementary effect on A2 coupling agent. In terms of comprehensive performance and added amount, test 4 is the best. The addition amount of A2 coupling agent is 2.5%, and the addition amount of A3 coupling agent is 2%. The intact rate of the paint film in the adhesion performance test can reach 95%, and the proportion of yellow iodine residue in the iodine resistance performance test is 3%. While meeting the performance requirements, the addition amount of A2 and A3 coupling agents is still the lowest, which makes the cost optimal. Therefore, the addition amount of A2 coupling agent is determined to be 2.5% and the addition amount of A3 coupling agent is determined to be 2%.

[0110] The test results are consistent with the design ideas. This formula not only achieves the requirement of improving the interlayer bonding strength, but also meets the function of resisting iodine penetration. Combined with the material cost price, the final product formula of test group 4 was selected, in which the addition amount of A2 coupling agent was 2.5% and the addition amount of A3 coupling agent was 2%.

[0111] 3. Waterborne polyurethane coating for elastic base surface protection and preparation method

[0112] 1. Coating formula

[0113] The present invention comprises component A and component B used in combination, wherein the components of component A are shown in Table 13, and the components of component B are shown in Table 14:

[0114] Table 13 Ingredients of Component A

[0115] Serial number Raw material name Components content 1 Deionized water water 18.5% 2 The first water-based acrylic resin Waterborne hydroxyl functional polyacrylate dispersion 35% 3 Second water-based acrylic resin Anionic polyacrylate dispersion 35% 4 Wetting Agents(349) Polyether modified polydimethylsiloxane 1.5% 5 Defoaming agent (901W) Polyether siloxane copolymer 1.5% 6 Thickener RM-8W Water-based nonionic associative polyurethane 1% 7 Thickener RM-5000 Solvent-free nonionic associative polyurethane 1% 8 A1 Surfactant Polyether siloxane copolymer 2% 9 A2 coupling agent Waterborne silane accelerator 2.5% 10 A3 coupling agent Silane compounds containing epoxy groups 2%

[0116] Table 14 Ingredients of component B

[0117]

[0118] Among them, the first water-based acrylic resin makes the paint film have high gloss and acid, alkali and other chemical resistance after completion, and the second water-based acrylic resin makes the paint film have better mechanical resistance, weather resistance and toughness after completion.

[0119] Preferably, the product model of the first water-based acrylic resin is Bayhydrol A 2770, and the product model of the second water-based acrylic resin is Bayhydrol A 2646.

[0120] 2. Preparation method of the coating

[0121] A method for preparing component A in a waterborne polyurethane coating for elastic base surface protection, the specific steps are as follows:

[0122] The first step is to add the formula deionized water, the first water-based acrylic resin and the second water-based acrylic resin at a speed of 600 r / min and disperse for 5 minutes;

[0123] The second step is to add wetting agent and defoamer at a speed of 1200r / min and disperse for 15 minutes;

[0124] The third step is to add thickener, polyether siloxane copolymer, water-based silane accelerator and epoxy-containing silane compound at a speed of 1200 r / min and disperse for 30 minutes;

[0125] The fourth step is testing, filtering and packaging.

[0126] 3. Usage and construction technology

[0127] First, stir the topcoat component A evenly, then pour in component B, use an electric stirrer to stir for 3 minutes until it is evenly mixed, then pour into another container and continue stirring for 2 minutes.

[0128] The surface layer is constructed by roller, and needs to be rolled twice, with an interval of 24-48 hours between each coating. The second coating can be carried out only after the first coating is dry. In addition, the site should be fully closed during the surface layer construction, and personnel management should be done well. The surface layer construction workers should wear dust-free clothes to evenly coat and form the final surface. When applying the top coating, use a roller to evenly apply to form a continuous and uniform coating film. Pay attention to the coating thickness during construction, and do not allow it to drip or leak.

[0129] 4. National third-party testing of building materials

[0130] The system was tested by the National Building Materials Third-Party Testing Center. The test results are shown in Table 15:

[0131] Table 15 Test report results of National Building Materials Testing Center

[0132]

[0133]

[0134] According to the test results, it can be proved that the material of the present invention can meet the relevant performance indicators of plastic flooring in terms of physical properties and chemical properties.

[0135] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-based polyurethane coating for protecting elastic base surfaces, It is characterized in that It comprises component A and component B used in combination, wherein: The component A comprises a first water-based acrylic resin, a second water-based acrylic resin, a polyether siloxane copolymer, a water-based silane accelerator, a silane compound containing an epoxy group and coating auxiliary materials; The component B is a curing agent; The amount of the polyether siloxane copolymer added is not less than 2% of the total weight of the component A, the amount of the water-based silane accelerator added is not less than 2.5% of the total weight of the component A, and the amount of the epoxy-containing silane compound added is not less than 2% of the total weight of the component A; The first water-based acrylic resin is a water-based hydroxyl functional polyacrylate dispersion, the second water-based acrylic resin is an anionic polyacrylate dispersion, the first water-based acrylic resin is added in an amount of 35-40% of the total weight of the component A, and the second water-based acrylic resin is added in an amount of 35-40% of the total weight of the component A; The curing agent is a hydrophilic aliphatic polyisocyanate of hexamethylene diisocyanate.

2. The waterborne polyurethane coating for elastic base surface protection according to claim 1, It is characterized in that The addition amount of the polyether siloxane copolymer is 2%-5% of the total weight of the component A, the addition amount of the water-based silane accelerator is 2.5%-5% of the total weight of the component A, and the addition amount of the epoxy-containing silane compound is 2%-5% of the total weight of the component A.

3. The waterborne polyurethane coating for elastic base surface protection according to claim 1, It is characterized in that The first water-based acrylic resin is a water-based hydroxyl-functional polyacrylate dispersion, the second water-based acrylic resin is an anionic polyacrylate dispersion, the addition amount of the first water-based acrylic resin is 35% of the total weight of the component A, and the addition amount of the second water-based acrylic resin is 35% of the total weight of the component A.

4. The waterborne polyurethane coating for elastic base surface protection according to claim 1, It is characterized in that The coating auxiliary materials include a wetting agent, a defoaming agent, a thickener and deionized water. The percentage of each component added in the coating auxiliary materials to the total weight of component A is: Wetting agent 1-2%; Defoaming agent 1-2%; Thickener 2-3%; Deionized water 18-19%.

5. The waterborne polyurethane coating for elastic base surface protection according to claim 4, It is characterized in that The percentage of each component added in the coating auxiliary material to the total weight of component A is: Wetting agent 1.5%; Defoaming agent 1.5%; Thickener 2%; Deionized water 18.5%.

6. The waterborne polyurethane coating for elastic base surface protection according to claim 5, It is characterized in that The thickener comprises water-based nonionic associative polyurethane and solvent-free nonionic associative polyurethane, wherein the addition amount of the water-based nonionic associative polyurethane accounts for 1% of the total weight of component A, and the addition amount of the solvent-free nonionic associative polyurethane accounts for 1% of the total weight of component A.

7. A method for preparing a waterborne polyurethane coating for elastic base surface protection as claimed in any one of claims 1 to 6, It is characterized in that The preparation method of component A comprises the following specific steps: Add the formula deionized water, the first water-based acrylic resin and the second water-based acrylic resin, disperse at a speed of 600 r / min for 5 minutes; Add wetting agent and defoamer, speed 1200r / min, disperse for 15 minutes; Add thickener, polyether siloxane copolymer, water-based silane accelerator and epoxy-containing silane compound at a speed of 1200 r / min and disperse for 30 minutes; Among them, the addition amount of the polyether siloxane copolymer is not less than 2% of the total weight of the component A, the addition amount of the water-based silane accelerator is not less than 2.5% of the total weight of the component A, and the addition amount of the epoxy-containing silane compound is not less than 2% of the total weight of the component A.

Citation Information

Patent Citations

  • Aqueous two-component polyurethane topcoat coating and preparation method thereof

    CN106398503A

  • Water-based two-component polyurethane paint for galvanized plates and preparation method of water-based two-component polyurethane paint

    CN111087906A

  • Anti-stain and organic disinfection solvent-resistant hospital wall coating and preparation method thereof

    CN115216220A