Reflective cement mortar and reflective semi-flexible pavement material

By using reflective cement mortar and bright-colored materials in semi-flexible pavement, the problem of poor reflective performance of semi-flexible pavement is solved, the reflection coefficient and brightness of the pavement are significantly improved, safety hazards and energy waste are reduced, and waste glass is eliminated resource utilization.

CN116514464BActive Publication Date: 2024-10-11CHONGQING JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310471404.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-11
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The existing semi-flexible pavement has poor reflective performance, which results in reduced tunnel pavement brightness, increased safety hazards and energy waste.

Method used

Reflective cement mortar is used, which consists of cement, glass powder, zeolite powder and water-reducing agent. Bright materials are embedded in the base asphalt mixture to improve the reflective performance of the road surface. The specific ratio is 70 to 95 parts of cement and glass powder. 5 to 15 parts, 0 to 15 parts of zeolite powder, 0.3 to 0.5 parts of water reducing agent, 40 to 50 parts of water, and brightly colored materials are embedded on the surface of the base asphalt mixture to improve the reflective properties.

Benefits of technology

It significantly improves the reflective performance of semi-flexible pavement, with the reflection coefficient increased by about 4 times, reducing safety hazards and energy waste, realizing the resource utilization of waste glass, and reducing expansion reactions and bleeding problems through zeolite powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514464B_ABST
    Figure CN116514464B_ABST
Patent Text Reader

Abstract

The invention discloses a reflective cement mortar and a reflective semi-flexible pavement material, wherein the addition amount of each component of the reflective cement mortar is calculated by weight: 70-95 parts of cement, 5-15 parts of glass powder, 0-15 parts of zeolite powder, 0.3-0.5 parts of water reducer, and 40-50 parts of water. The semi-flexible pavement material comprises the above-mentioned reflective cement mortar, a base asphalt mixture and a bright color material, wherein the addition amount of the bright color material is 2-4wt% of the base asphalt mixture. The semi-flexible pavement material of the invention improves the reflective performance of the cement mortar by adding glass powder and zeolite powder; at the same time, the reflective performance of the base asphalt mixture is further improved by bright color paving. When the semi-flexible pavement is used in a tunnel, it can effectively reduce the safety hazards and energy waste of driving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a reflective cement mortar and a reflective semi-flexible pavement material. Background Art

[0002] Semi-flexible pavement is a composite pavement material that is both rigid and flexible, formed by pouring cement slurry into asphalt mixture. Compared with traditional asphalt pavement, semi-flexible pavement has the advantages of strong bonding ability, outstanding high temperature performance, stiffness, durability, and better resistance to rutting and pushing diseases. Therefore, semi-flexible pavement has been increasingly used.

[0003] However, when semi-flexible pavement is applied to tunnel pavement, since the surface of the semi-flexible pavement mainly contains asphalt, the black asphalt mixture has the characteristic of strong light absorption, which will absorb the surrounding light, making the pavement brightness lower, which is easy to cause safety hazards and energy waste. Therefore, it is urgent to provide a semi-flexible pavement with reflective properties to reduce safety hazards and energy waste. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a reflective cement mortar and a reflective semi-flexible pavement material to solve the problems that the existing semi-flexible pavements have poor reflective performance, are prone to safety hazards and waste of energy.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A reflective cement mortar, wherein the addition amount of each component is calculated by weight: including 70-95 parts of cement, 5-15 parts of glass powder, 0-15 parts of zeolite powder, 0.3-0.5 parts of water reducing agent, and 40-50 parts of water.

[0007] Preferably, the added amount of each component is calculated by weight: including 70-80 parts of cement, 10-15 parts of glass powder, 10-15 parts of zeolite powder, 0.4 parts of water reducing agent, and 45 parts of water.

[0008] More preferably, the added amount of each component is calculated by mass: 70 parts of cement, 15 parts of glass powder, 15 parts of zeolite powder, 0.4 parts of water reducing agent, and 45 parts of water.

[0009] Furthermore, the particle size of the glass powder is 0.1-0.2 mm, and the particle size of the zeolite powder is 0.05-0.1 mm.

[0010] A reflective semi-flexible pavement material is made by the following method: firstly, a base asphalt mixture is paved to form a macroporous base surface, and then a bright color material is paved on the base asphalt mixture in a surface-embedded manner, and after rolling or compacting, it is cured at room temperature for 24 hours; then, any of the reflective cement mortars is poured into the base asphalt mixture, and after curing at room temperature for 24 hours, the reflective semi-flexible pavement material is obtained. The amount of the bright color material added is 2-4wt% of the base asphalt mixture.

[0011] The light-colored material is white stone or waste glass with a particle size of 4.75 to 9.5 mm. When the light-colored material is white stone, the oil-stone ratio of the base asphalt mixture is 3.3 to 3.7%; when the light-colored material is waste glass, the oil-stone ratio of the base asphalt mixture is 3.4 to 3.7%.

[0012] The asphalt of the base asphalt mixture is styrene-butadiene-styrene modified asphalt.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The present invention provides a reflective cement mortar, which improves the reflective performance of the cement mortar by compounding glass powder, zeolite powder and cement; the raw materials are easily available, the cost is low, and the waste glass is recycled. In addition, the zeolite powder can not only improve the reflective performance by utilizing its own whiteness, but also reduce the expansion reaction caused by the addition of glass powder, and improve the bleeding and segregation problems caused by the addition of glass powder; in addition, the zeolite powder can also effectively improve the workability of the cement mortar, so that the glass powder can be more evenly distributed in the cement mortar, making the road surface reflective performance more uniform.

[0015] 2. The reflective cement mortar of the present invention is used for the semi-flexible pavement in the tunnel, and the reflective performance of the semi-flexible pavement is further improved by embedding bright color materials on the surface of the base asphalt mixture. The average brightness of the reflective semi-flexible pavement is about 4 times higher than that of the traditional AC-13 pavement, and the reflection coefficient is as high as 0.192. The semi-flexible pavement material of the present invention is made by pouring reflective cement mortar, which is of great significance for improving the reflective performance of the pavement, reducing safety hazards and energy waste.

[0016] 3. The present invention also studies the influence of different types, dosages and particle sizes of bright color materials on the reflective performance of the road surface, thereby determining the best bright color paving scheme. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A comparison diagram of solar radiation reflectivity of reflective cement mortars of Examples 1 to 6 of the present invention and existing cement mortars;

[0018] Figure 2The present invention is a flow chart for preparing the reflective semi-flexible pavement;

[0019] Figure 3 The average illumination diagram of the reflective semi-flexible pavement materials obtained in Examples 7-16 of the present invention and the conventional asphalt mixture pavement AC-13 of the comparative example in the tunnel model;

[0020] Figure 4 The average brightness diagram of the reflective semi-flexible pavement materials obtained in Examples 7-16 of the present invention and the conventional asphalt mixture pavement AC-13 of the comparative example in the tunnel model;

[0021] Figure 5 Graph showing the reflection coefficients of the reflective semi-flexible pavement materials obtained in Examples 7-16 of the present invention and the conventional asphalt mixture pavement AC-13 of the comparative example in a tunnel model. DETAILED DESCRIPTION

[0022] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.

[0023] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.

[0024] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.

[0025] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.

[0026] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods.

[0027] The quantitative tests in the present invention were all repeated three times, and the results were averaged.

[0028] 1. A reflective cement mortar

[0029] The invention comprises the following components, calculated by weight: 70-95 parts of cement, 5-15 parts of glass powder, 0-15 parts of zeolite powder, 0.3-0.5 parts of water reducing agent and 40-50 parts of water.

[0030] Among them, cement is one of the main ingredients of cement grouting material. Common cement in this field can be used, but silicate cement is preferred; cement is an important guarantee for the mechanical strength of reflective mortar to meet the requirements. The addition of cement plays a decisive role in improving the mechanical strength of reflective mortar, and after cement hydration, it will provide a good alkaline environment for the volcanic ash reaction of fly ash, which can realize resource recycling.

[0031] Glass powder is obtained by grinding waste glass or white stones after crushing. The raw material source is easy to obtain, and the waste glass is recycled. Glass powder is a bright material, but the silica content in glass is high. When glass is used in cement concrete, the alkali in the concrete reacts with free silicon to form alkali silica gel, and an ASR expansion reaction will occur as shown in formula (1):

[0032] SiO2+2Na + (K + )+2OH — →Na2(K2)SiO3H2O (1)

[0033] This makes the expansion rate of cement concrete too high and the road performance deteriorates. Therefore, the particle size of glass powder is controlled at 0.1-0.2 mm.

[0034] Zeolite is a framework-structured hydrated aluminum silicate mineral. Due to its volcanic ash properties, it is widely used as a supplementary cementitious material. The unsaturated zeolite structure can absorb alkaline ions in concrete and reduce the alkalinity of the concrete pore solution, thereby reducing ASR expansion. Prevent destructive intercalation between the interface between cement mortar and asphalt mixture. In the experiment, it was found that cement mortar with glass powder instead of cement is prone to bleeding and segregation, while zeolite powder with a porous structure has good water retention and can effectively improve the problems of bleeding and segregation. The average particle size of zeolite powder should be controlled at 0.05-0.1mm.

[0035] The water reducer is preferably polycarboxylic acid. When the water amount is unchanged, adding an appropriate amount of water reducer will not affect the mechanical properties of the mortar and can also prepare a mortar with good fluidity. At the same time, the gelling material inside the mortar can also be more evenly dispersed in the slurry.

[0036] 2. Reflective Cement Mortar Embodiment

[0037] The raw material proportions of Examples 1 to 5 and Comparative Example are shown in Table 1.

[0038] Table 1 Raw material ratio table of reflective cement mortar of Examples 1-5 and comparative example cement mortar (parts by weight)

[0039] Example cement Glass powder Zeolite powder water Water reducing agent 28d expansion rate % Example 1 95 5 0 45 0.4 0.012 Example 2 90 10 0 45 0.4 0.05 Example 3 85 10 5 45 0.4 0.036 Example 4 80 10 10 45 0.4 0.03 Example 5 70 15 15 45 0.4 0.025 Example 6 90 0 10 45 0.4 / Comparative Example 100 0 0 45 0.4 /

[0040] The preparation method of the reflective cement mortar comprises the following steps:

[0041] (1) Weigh cement, glass powder, zeolite powder and water reducer according to the proportion, pour into the mixing pot, and stir with a machine for 60 seconds until it is uniform and without stratification.

[0042] (2) Add the weighed water into the mixing pot of the uniformly stirred cementitious material, stir manually for about 60 seconds until it is uniform and free of lumps, and then use a machine to stir for 60 seconds to obtain the reflective slurry.

[0043] Since the semi-flexible pavement material requires a very high fluidity of the mortar, direct stirring by machine is likely to cause splashing of the mortar, resulting in loss of the reflective mortar. Therefore, the present invention performs manual stirring before machine stirring.

[0044] From the comparison between Example 1 and Example 2, it can be seen that with the increase of glass powder, the expansion rate of cement mortar increases; and from the comparison between Examples 2 to 4, it can be seen that with the increase of zeolite powder content, the expansion rate of cement mortar gradually decreases, indicating that the addition of zeolite powder can effectively inhibit the expansion of cement mortar caused by the addition of glass powder, thereby preventing the destructive interlocking effect between the interface between cement mortar and asphalt mixture.

[0045] Figure 1 This is a comparison chart of the solar radiation reflectivity of the reflective cement mortars of Examples 1 to 6 of the present invention and the existing cement mortar ( Figure 1 Where B represents glass powder, F represents zeolite powder, and the numbers after B and F represent the amount of the corresponding substances added). Figure 1 It can be seen that with the increase of glass powder content, the reflectivity of cement mortar gradually increases. It can be seen that adding glass powder to cement mortar can significantly improve the reflectivity of cement mortar. When it is applied to semi-flexible pavement, it can reduce the safety hazards of tunnel driving and unnecessary energy waste. At the same time, the reuse of waste glass is of great significance for resource recycling and environmental protection.

[0046] When the content of glass powder or white stone is certain, with the increase of zeolite powder, the reflection first decreases and then increases. The inventor analyzed that the reason may be: glass powder is prone to stratification and segregation in cement slurry with greater fluidity, and some glass powder is not evenly dispersed in the cement slurry, but precipitated on the surface, while zeolite powder can effectively improve the workability of cement slurry, so that the glass powder can be more evenly distributed inside the cement slurry, so when zeolite powder is first added, its reflectivity decreases instead. The whiteness of zeolite powder is relatively high. With the increase of zeolite dosage, the color of mortar becomes lighter, which can also play a role in improving the reflectivity. Therefore, the reflectivity gradually increases with the increase of zeolite powder. It can be seen that the addition of zeolite powder can not only enhance the reflectivity of cement mortar, but also enhance the workability of glass powder, so that it can be evenly dispersed in cement mortar, thereby enhancing the reflective performance of pavement materials.

[0047] When 10 parts of zeolite powder are added alone, the reflectivity is equivalent to the reflectivity of 5 parts of glass powder added alone, which shows that the reflective performance of glass powder is significantly better than that of zeolite powder. In addition, by using waste glass as the main reflective material, the waste glass can be reused at a lower cost. Therefore, the reflective mortar of the present invention mainly uses glass powder as the reflective material.

[0048] 3. A reflective semi-flexible pavement material

[0049] See also Figure 2 A reflective semi-flexible pavement material, the preparation method of which comprises the following steps: firstly paving a base asphalt mixture into a large-pore base surface, then paving a bright-colored material on the base asphalt mixture in a surface-embedded manner, rolling or compacting it, and curing it at room temperature for 24 hours; then pouring the reflective cement mortar of the present invention into the base asphalt mixture, and curing it at room temperature for 24 hours to obtain the reflective semi-flexible pavement material.

[0050] The amount of the bright color material added is 2-4wt% of the base asphalt mixture. The void ratio of the base asphalt mixture is 20-30%. The bright color material is waste glass blocks or white stones with a particle size of 4.75-9.5mm.

[0051] When the bright material is waste glass blocks, the asphalt-to-rock ratio of the base asphalt mixture is 3.4-3.7%. Considering the cost factor, the preferred asphalt-to-rock ratio is 3.4%.

[0052] When the light-colored material is white stone, the asphalt-to-stone ratio of the base asphalt mixture is 3.3-3.7%. Considering the cost factor, the preferred asphalt-to-stone ratio is 3.3%.

[0053] 4. Embodiment of reflective semi-flexible pavement material

[0054] Examples 7-16 are preferred embodiments of reflective semi-flexible pavement materials. When the base asphalt mixture and the reflective mortar are the same, a comparison table of the types, particle sizes and amounts of the bright color materials in Examples 7-16 is shown in Table 2.

[0055] Table 2 Comparison of types, particle sizes and amounts of bright color materials

[0056]

[0057]

[0058] Note: S─white stone; B─waste glass; A─the amount of single particle size light-colored material added is 2%; C─the amount of single particle size light-colored material added is 4%; D─the sum of the amounts of two particle size light-colored materials added is 4%.

[0059] 5. Evaluation of reflective performance of semi-flexible reflective pavement materials

[0060] In order to restore the actual tunnel project, the present invention conducts a reflective performance test in a self-made simple tunnel model to study the influence of different reflective semi-flexible pavement materials on the average brightness, average illumination and reflection coefficient of the tunnel pavement. The reflective semi-flexible pavement materials used in the experiment are the reflective semi-flexible pavement materials obtained in Examples 7-16 and the comparative example traditional asphalt mixture pavement AC-13.

[0061] The average road surface illumination refers to the average illumination of each point measured or calculated on the road surface. The illumination calculation formula is as follows:

[0062] E=dΦ / dA

[0063] Where: E is the illuminance value at a point on the target surface (lx); dΦ is the luminous flux on the surface containing the point (lm); dA is the area of ​​the surface element (m 2 )

[0064] The average road surface brightness can be obtained by measuring or calculating the average brightness of each point on the road surface at a predetermined point.

[0065] The brightness calculation formula is as follows:

[0066] L=dΦ / (dA·θ·dΩ)

[0067] Where, L—brightness (cd / m 2 );dΦ—luminous flux of the beam element at the test point propagating within the solid angle element dΩ in the test direction (lm);θ—angle between the test beam direction and the cross-section normal (°); dA—beam cross-sectional area at the test point (m 2 );dΩ—cubic angle element in the test direction (sr).

[0068] The reflection coefficient refers to the ratio of the reflected luminous flux to the incident luminous flux under the specified conditions of the spectral composition, polarization state and geometric distribution of the incident light. It can be obtained by converting between brightness and illuminance. The "Lighting Measurement Method" stipulates that the road surface material is a diffuse reflection material, and the calculation formula for the reflection coefficient is as follows:

[0069] ρ=πL / E

[0070] ρ—road surface reflection coefficient; L—road surface brightness, in candela per square meter (cd / ㎡); E—road surface illumination, in lux (lx).

[0071] 1. Average road illumination

[0072] Figure 3 This is the average illumination diagram of the reflective semi-flexible pavement materials obtained in Examples 7-16 and the comparative example traditional asphalt mixture pavement AC-13 in the tunnel model. Figure 3 Among them, (a) is the average illumination diagram of semi-flexible pavement materials of various bright colors; (b) is the average illumination diagram of glass-type semi-flexible pavement materials; (c) is the average illumination diagram of white stone-type semi-flexible pavement materials.

[0073] Depend on Figure 3 (a) It can be seen that compared with the traditional AC-13 pavement material, the reflective semi-flexible pavement materials of the present invention have a significant effect on improving the average illumination in the tunnel, which is related to the reflective cement mortar in the structural seams of the semi-flexible pavement material itself. Among them, the improvement of the average illumination by white stone-like bright-color materials is slightly higher than that of glass-like bright-color materials. The reason may be that the transparent glass blocks on the asphalt mixture with a black base color still make the overall color darker and the light absorption rate is still very large. Therefore, even if the glass blocks have a better mirror reflection surface, the effect of using them in asphalt pavement is still not as good as that of white stones.

[0074] Depend on Figure 3 (b) It can be seen that as the amount of glass-like bright-color materials embedded on the surface increases, the average illumination in the tunnel environment increases, but the relationship between the change in particle size of glass-like bright-color materials and the change in average illumination cannot be clearly observed;

[0075] Depend on Figure 3 (c) It can be seen that the ambient illumination of white stone-like bright-color materials will not only increase with the increase of embedded amount, but also increase with the increase of particle size. The reason is that large stones are smoother per unit area than small stones, and their specular reflection is stronger.

[0076] 2. Average road brightness

[0077] Figure 4This is a graph showing the average brightness of the reflective semi-flexible pavement materials obtained in Examples 7-16 and the comparative example conventional asphalt mixture pavement AC-13 in a tunnel model. Figure 4 Among them, (a) is the average brightness diagram of semi-flexible pavement materials of various bright colors; (b) is the average brightness diagram of glass-type semi-flexible pavement materials; (c) is the average brightness diagram of white stone-type semi-flexible pavement materials.

[0078] Depend on Figure 4 (a) It can be seen that the reflective semi-flexible pavement material significantly improves the brightness of the road surface in the tunnel. When the white stone embedding amount is 4% and the particle size is 9.5mm, the reflective semi-flexible pavement increases the average brightness by 4 times compared with the AC-13 pavement; when the glass block embedding amount is 2% and the particle size is 4.75mm, the average brightness of the reflective semi-flexible pavement is relatively weak, but it is also increased by about 3 times compared with the average brightness of the AC-13 pavement. In addition, according to Figure 4 (a) It can also be found that the improvement of average brightness by white stone-like bright-color materials is slightly higher than that by glass-like bright-color materials.

[0079] Depend on Figure 4 (b) It can be seen that the variation pattern of the average brightness of glass-like bright-color materials is similar to the average illumination, which increases with the increase of the embedded amount and has no obvious relationship with the particle size;

[0080] Depend on Figure 4 (c) It can be seen that the variation pattern of the average brightness of white stone-like bright-color materials is similar to the average illumination, and increases with the increase of the embedded amount and particle size of the bright-color materials.

[0081] 3. Road surface reflection coefficient

[0082] Figure 5 The reflection coefficient diagram of the reflective semi-flexible pavement material obtained in Examples 7-16 and the conventional asphalt mixture pavement AC-13 in the tunnel model is shown in FIG. Figure 5 It can be seen that the reflective semi-flexible pavement material significantly improves the pavement reflection coefficient. When the glass embedding amount of the glass-type reflective semi-flexible pavement material is 4% and the particle size is 9.5mm, the pavement reflection coefficient is increased from 0.048 of AC-13 to 0.156; and for the white stone-type reflective semi-flexible pavement material, when the embedding amount is 4% and the particle size is 9.5mm, the reflection coefficient can be as high as 0.192. The change law is consistent with the average illumination and average brightness. The reflection coefficient of the pavement material is proportional to the embedding amount of the bright color material, and the larger the particle size of the bright color material, the smoother the pavement is, so the reflection coefficient is higher.

[0083] In summary, the use of the reflective semi-flexible pavement material of the present invention for paving the road surface in the tunnel can significantly improve the illumination, brightness and reflection coefficient of the road surface, which is of great significance for improving the reflective performance of the road surface in the tunnel, reducing safety hazards and saving energy.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A reflective cement mortar, characterized in that: The addition amount of each component is calculated according to the following mass parts: cement 70-80 parts, glass powder 10-15 parts, zeolite powder 10-15 parts, water reducer 0.4 parts, water 45 parts; The particle size of the glass powder is 0.1-0.2 mm, and the particle size of the zeolite powder is 0.05-0.1 mm.

2. The reflective cement mortar according to claim 1, characterized in that: The added amount of each component is calculated according to the following mass parts: 70 parts of cement, 15 parts of glass powder, 15 parts of zeolite powder, 0.4 parts of water reducing agent, and 45 parts of water.

3. A reflective semi-flexible pavement material, characterized in that: The method is as follows: first, a base asphalt mixture is paved into a large-pore base surface, and then a bright-colored material is paved on the base asphalt mixture in a surface-embedded manner, and after rolling or compacting, it is cured at room temperature for 24 hours; then, the reflective cement mortar described in claim 1 or 2 is poured into the base asphalt mixture, and after curing at room temperature for 24 hours, a reflective semi-flexible pavement material is obtained; The amount of the light-colored material added is 2-4wt% of the base asphalt mixture; the light-colored material is white stone or waste glass with a particle size of 4.75-9.5mm.

4. The reflective semi-flexible pavement material according to claim 3, characterized in that: When the light-colored material is white stone, the oil-stone ratio of the base asphalt mixture is 3.3-3.7%; when the light-colored material is waste glass, the oil-stone ratio of the base asphalt mixture is 3.4-3.7%.

5. The reflective semi-flexible pavement material according to claim 3, characterized in that: The asphalt of the base asphalt mixture is styrene-butadiene-styrene modified asphalt.