Glass powder, conductive copper paste, multilayer ceramic capacitor and preparation method for MLCC
By using boron-zinc-silicon system glass powder in the MLCC copper terminal slurry and doping with CuO, TiO2, and ZrO2, combined with the integrated sintering and crystallization process, the problems of poor high-temperature wettability and poor acid resistance of the glass powder are solved, and MLCC is realized The high density and acid resistance of the copper terminal electrode improve the overall performance of the device.
Patent Information
- Application Number
- CN202310503457.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-04-28
AI Technical Summary
In the prior art, the glass powder used for MLCC copper terminal slurry has poor high-temperature wettability, poor acid resistance, and low sintering density. This results in the terminal electrodes having non-dense copper powder and easy oxidation during the sintering process, and the plating layer moves toward the terminal electrode during the electroplating process. The diffusion of terminal electrodes limits the application of MLCC.
Using boron-zinc-silicon system glass powder, doped with CuO, TiO2 and ZrO2, the glass powder is optimized through low melting point and high-temperature fluidity, combined with the integrated sintering and crystallization process, to form a copper terminal with excellent acid resistance, low porosity and dense sintering electrode.
It effectively reduces the sintering temperature of the glass powder, improves the acid resistance and density of the copper terminal electrode, avoids cracks and crack defects during the electroplating process, and has a simple process and high efficiency.
Smart Images

Figure CN116535097B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of capacitors, and in particular to a glass powder, a conductive copper paste, a multilayer ceramic capacitor and a preparation method thereof for MLCC. Background Art
[0002] Looking at the development of modern electronic devices in recent decades, multilayer ceramic capacitors (MLCC) have gradually become an irreplaceable and important component in the historical development of electronic devices. MLCC is also well-known and widely used due to its wide temperature range, wide capacitance range, low dielectric loss, high stability, suitability for automated plug-in production and relatively low price.
[0003] MLCC is composed of ceramic dielectric, internal electrode and terminal electrode, and the low-temperature sintered copper electronic paste used to prepare the terminal electrode is mainly composed of metal copper powder, inorganic glass powder and organic carrier. Among them, glass powder plays a decisive role as a bonding phase. The characteristics of MLCC terminal electrodes place high demands on the adhesion, acid resistance and sintering density of glass powder. At present, the glass powder used to prepare electrode slurry generally has the disadvantages of high Tg point, poor high-temperature wettability, poor corrosion resistance of electroplating solution and low sintering density. These shortcomings will cause the copper powder of the terminal electrode to be not dense and easy to oxidize during the sintering process, and the plating layer will diffuse to the terminal electrode during the electroplating process. The above phenomenon greatly limits the application of MLCC.
[0004] Traditionally, low-melting-point glasses used for MLCC copper terminal electrodes include barium borosilicate glass and boron zinc silicon glass, which have relatively good wettability with copper, but weak acid resistance and require high temperature to form a sintered dense film. Chinese Patent 202110994508.8 introduces a high sintering density copper paste for MLCC and a preparation method thereof. The components in the copper paste formula described in the invention are as follows by mass percentage: first copper powder 40-60%; second copper powder 10-30%; first glass powder 3-5%; second glass powder 0.5-2.5%; organic carrier 20-25%; and, additive 0.5-3%. The invention uses two systems of glass powder for compounding, which can effectively optimize the nickel penetration phenomenon during electroplating and improve the reliability of MLCC products. At the same time, the sintering temperature of the copper paste can be reduced in the process to save energy. However, judging from the example figure, the sintering density of its copper terminal electrode still needs to be improved. CN113724912A discloses a high sintering density copper paste for MLCC and a preparation method thereof, which further discloses that the components in the copper paste formula are as follows by mass percentage: 40-60% of the first copper powder; 10-30% of the second copper powder; 3-5% of the first glass powder; 0.5-2.5% of the second glass powder; 20-25% of the organic carrier; and 0.5-3% of the auxiliary agent; wherein the first copper powder and the second copper powder are spherical copper powders, and the average particle size of the first copper powder is larger than the average particle size of the second copper powder. By selecting a suitable type of copper powder, the density of the sintered rear end electrode is improved, but it cannot solve the bubbling problem on the side or the top and the appearance problem of edge cracking caused by excessive sintering shrinkage between the edge copper powders during sintering. Chinese patent 202210550568.5 discloses a glass powder for low-temperature sintering MLCC terminal electrode slurry and its preparation method. The glass powder raw material composition is: 10% to 40% B2O3, 20% to 50% BaO, 5% to 20% ZnO, 2% to 15% SiO2, 1% to 5% Al2O3, 10% to 40% TeO2. The glass powder provided by the invention does not contain lead toxic elements, and the sintering temperature is 650 to 750 ° C. After the glass powder is sintered, it has good wettability and strong adhesion with the MLCC ceramic matrix. The sintered terminal electrode is dense, and there is no cracking and etching after corrosion by the electroplating solution. It has good corrosion resistance and stable chemical properties. However, the glass powder in the invention contains Te elements, which is relatively expensive and may have a negative impact on the structure and performance of the copper terminal electrode. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, propose a glass powder, conductive copper paste, multilayer ceramic capacitor and preparation method for MLCC, and solve the technical problems of poor high-temperature wettability, poor acid resistance and low sintering density of the glass powder used for MLCC copper end paste in the prior art.
[0006] In the first aspect, the present invention provides a glass powder for MLCC, the raw materials of which include: a basic glass component and an external doping component; wherein the basic glass component is a boron zinc silicon system glass, the external doping component is CuO, TiO2 and ZrO2, and the mass ratio of the basic glass component to CuO, TiO2 and ZrO2 is 100: (0.5~1.5): (0.5~1.5): (0.5~1.5).
[0007] In a second aspect, the present invention provides a method for preparing a glass powder for MLCC, comprising the following steps:
[0008] Weighing and grinding the raw materials of the basic glass component and the externally added component into a raw material solid powder;
[0009] Sintering raw material solid powder into glass liquid;
[0010] Pour the glass liquid into cold water for quenching, and crush it into glass particles after cooling;
[0011] The glass particles are ball-milled and sieved in sequence to obtain glass powder.
[0012] In a third aspect, the present invention provides a conductive copper paste for MLCC, the raw materials of which include: copper powder, an organic carrier and the glass powder for MLCC provided in the first aspect of the present invention.
[0013] In a fourth aspect, the present invention provides a multilayer ceramic capacitor, comprising: a ceramic body and a copper end electrode, and the copper end electrode is obtained by applying the conductive copper paste for MLCC provided by the third aspect of the present invention to both ends of the ceramic body and then subjecting the ceramic body to an integrated sintering and crystallization treatment.
[0014] Compared with the prior art, the beneficial effects of the present invention include:
[0015] The boron zinc silicon system glass powder prepared by the present invention contains CuO, TiO2 and ZrO2. Copper ions act as the outer body of the glass in the glass structure. The boron zinc silicon system glass powder with CuO added can effectively reduce its sintering temperature. At the same time, TiO2 and ZrO2 are added, and ZnB2O4 crystals are precipitated after integrated sintering, which can effectively avoid the defects such as cracks and cracks caused by the acidic plating solution in the electroplating process of the MLCC terminal electrode. The glass powder has the characteristics of low glass transition temperature (Tg) and excellent high-temperature fluidity. At the same time, the conductive copper paste formed by mixing the glass powder with copper powder and organic carrier, combined with the copper terminal electrode prepared by the integrated sintering and crystallization process of the present invention, has the advantages of excellent acid resistance, low porosity and high sintering densification, and the internal stress of the MLCC device is moderate and evenly distributed after sintering. The glass powder, conductive copper paste and copper terminal electrode of the present invention also have the advantages of simple preparation process and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is the sintering wetting angle of the glass powder prepared in Comparative Example 1 and Examples 1 to 3 of the present invention; wherein, Comparative Example 1 is 45.8°, Example 1 is 59.6°, Example 2 is 56.6°; and Example 3 is 53.4°;
[0017] Figure 2 is the XRD pattern of the glass powder prepared in Examples 1 to 3 of the present invention;
[0018] Figure 3 The SEM characterization image of the glass obtained by heat treatment of the glass powder obtained in Examples 1 to 3 of the present invention and Comparative Example 1 through the same sintering system as the copper terminal electrode after acid etching;
[0019] Figure 4 This is a SEM characterization image of the sintering density of the copper terminal electrode prepared in Example 1 of the present invention;
[0020] Figure 5 is the porosity of the copper terminal electrode prepared in Examples 1 to 3 of the present invention;
[0021] Figure 6 is a diagram showing the distribution of internal stress of the copper terminal electrode prepared in Example 1 of the present invention;
[0022] Figure 7 This is the EDS scanning spectrum of the cross section of the copper terminal electrode prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0024] In a first aspect, the present invention provides a glass powder for MLCC, the raw materials of which include: a basic glass component and an externally doped component; wherein the basic glass component is a boron-zinc-silicon system glass, and the externally doped component is CuO, TiO2 and ZrO2.
[0025] Boron-zinc-silicon system glass is widely used in the preparation of MLCC copper-end slurry due to its low Tg point, good high-temperature fluidity, low melting temperature and cheap and readily available raw materials. However, as a bonding phase in the slurry, boron-zinc-silicon system glass also has the problems of poor acid resistance and low sintering density. In order to optimize the acid resistance, high-temperature wettability and sintering density of the boron-zinc-silicon system glass powder, the present invention adds a small amount of CuO to reduce the sintering temperature and optimize the high-temperature wettability, and adds TiO2 and ZrO2 as nucleating agents. The optimized glass powder of the present invention has the advantages of low melting point, good high-temperature wettability, excellent acid resistance and high sintering density, so that the glass powder has the potential to be used in the sintering preparation process of MLCC copper-end electrodes. After the optimized glass powder is sintered together with copper powder, ZnB2O4 crystals can be precipitated, which is beneficial to improve the acid resistance and density of the copper-end electrode.
[0026] In this embodiment, the basic glass composition is composed of the following components in terms of mass percentage of oxides: B2O3 10-50%, ZnO 10-50%, SiO2 5-40%, Al2O3 1-20%, Na2O 1-10%, Li2O 1-10%, BaO 1-10%.
[0027] In some specific embodiments of the present invention, the basic glass component is composed of the following components in terms of mass percentage of oxides: B2O3 10-40%, ZnO 40-50%, SiO2 10-25%, Al2O3 2-6%, Na2O 1-3%, Li2O 1-3%, BaO 3-6%.
[0028] In this embodiment, the mass ratio of the basic glass component to CuO, TiO2 and ZrO2 is 100: (0.5-1.5): (0.5-1.5): (0.5-1.5), and further 100: (0.5-1.5): 1: 1. The inventors found in the experimental process that the high-temperature fluidity (wettability) of the glass will only suddenly decrease in the process of "from scratch" of copper oxide, while the wettability of the glass will continue to increase with the continuous increase of the copper oxide content. It can be seen that in the glass powder system of the present invention, copper oxide can optimize the high-temperature fluidity of the glass and is beneficial to improve the sintering matching of the glass and copper powder; however, excessive amount will cause the glass to be unable to wrap and adhere to the copper powder particles after high-temperature melting, resulting in device surface defects and poor sintering matching of the glass and copper powder. However, if the content of Ti and Zr as nucleating agents is too low, the glass will not be able to crystallize or the amount of crystallization will be too low and the acid resistance will be insufficient. If the content is too high, the end faces will be covered by ZnB2O4 crystals, affecting the electrical properties of the device. Sometimes it will even lead to phase separation during the glass melting preparation process, and the raw materials cannot be completely melted to form molten glass.
[0029] In a second aspect, the present invention provides a method for preparing a glass powder for MLCC, comprising the following steps:
[0030] Step S1, weighing the raw materials of the basic glass component and the external component, grinding and mixing them into raw material solid powder;
[0031] Step S2, sintering the raw material solid powder into glass liquid;
[0032] Step S3, pouring the glass liquid into cold water for quenching, and crushing it into glass particles after cooling;
[0033] Step S4, ball-milling and sieving the glass particles in sequence to obtain glass powder.
[0034] In this embodiment, during the process of sintering the raw solid powder into glass liquid, the heating rate is 2-10°C / min, further 5°C / min; the firing temperature is 900-1200°C, further 1000°C, and the firing time is 10-60min, further 30min.
[0035] In this embodiment, a ball mill is used for ball milling, the speed of the ball mill is 300-600r / min, further 400-440r / min, and the ball milling time is 30-300min. In some specific embodiments of the present invention, ball milling includes coarse grinding and fine grinding. During the coarse grinding process, the ball milling time is 60-180min, further 120min. During the fine grinding process, alcohol needs to be added as a ball milling medium, and the mass ratio of alcohol to glass powder is 1: (0.5-2), further 1: 1; the ball milling time is 30-120min, further 80min. After the fine grinding is completed, drying treatment is required before screening to volatilize the alcohol.
[0036] In this embodiment, during the screening process, the mesh size of the screen is 200 to 300 meshes.
[0037] In a third aspect, the present invention provides a conductive copper paste for MLCC, the raw materials of which include: copper powder, an organic carrier and the glass powder for MLCC provided in the first aspect of the present invention.
[0038] The conductive copper paste of the present invention uniformly precipitates ZnB2O4 crystals in the glass phase after sintering, so that the acid resistance and compactness of the glass phase change, and the acid resistance and compactness of the copper terminal electrode are effectively improved.
[0039] The present invention does not limit the type of copper powder, and those skilled in the art can select according to actual conditions. For example, it can be spherical copper powder or flake copper powder. In some specific embodiments of the present invention, spherical copper powder purchased from Guangbo Company is used.
[0040] In this embodiment, the organic carrier includes a resin and an organic solvent. Among them, the resin accounts for 4% to 10% of the mass percentage of the organic carrier; the organic solvent accounts for 90% to 96% of the mass percentage of the organic carrier; the resin is at least one of ethyl cellulose, cellulose acetate butyrate, and acrylic resin; the organic solvent is at least one of acetone, turpentine, terpineol, dihydroterpineol, ethylene glycol butyl ether, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, tributyl citrate, and dibutyl phthalate. In some specific embodiments of the present invention, the organic carrier is prepared by mixing diethylene glycol butyl ether, terpineol, and ethyl cellulose in a mass ratio of 48:48:4.
[0041] In this embodiment, the conductive copper paste used for MLCC includes, by mass percentage, 70-85% copper powder, 10-25% organic vehicle, and 4-10% glass powder.
[0042] In some specific embodiments of the present invention, the conductive copper paste for MLCC comprises, by mass percentage, 76% copper powder, 20% organic carrier, and 4% glass powder.
[0043] In a fourth aspect, the present invention provides a multilayer ceramic capacitor, comprising: a ceramic body and a copper end electrode, and the copper end electrode is obtained by applying the conductive copper paste for MLCC provided by the third aspect of the present invention to both ends of the ceramic body and then subjecting the ceramic body to an integrated sintering and crystallization treatment.
[0044] The conductive copper paste is prepared from the glass powder provided by the first aspect of the present invention, and the copper terminal electrode is prepared in combination with the integrated sintering and crystallization process of the present invention, which has the advantages of excellent acid resistance, low porosity and high sintering densification. After sintering, the internal stress of the MLCC device is moderate and evenly distributed. Compared with the traditional sintering process, the process is more simplified.
[0045] In this embodiment, during the integrated sintering and crystallization process, the temperature is raised to 700-850°C at a heating rate of 1-10°C / min and kept at that temperature for 10-50 minutes. In some specific embodiments of the present invention, the heating rate is 5°C / min, the maximum sintering temperature is 750°C, and the holding time is 15 minutes.
[0046] The present invention does not limit the type of ceramic body, and those skilled in the art can select it according to actual conditions, for example, it can be a BaTiO3 ceramic body.
[0047] In the following embodiments and comparative examples of the present invention, unless otherwise specified, some raw materials are summarized as follows:
[0048] The copper powder is spherical copper powder from Guangbo Nano New Materials Co., Ltd., with an average particle size of 3 μm;
[0049] The organic carrier is prepared by mixing diethylene glycol butyl ether, pinene alcohol and ethyl cellulose in a mass ratio of 48:48:4;
[0050] The ceramic body is a BaTiO3 ceramic body.
[0051] Example 1
[0052] (1) B2O3, ZnO, SiO2, Al2O3, Na2O, Li2O and BaO powders were weighed in a mass percentage of 38:40:13:2:1.5:1.5:4, ground and mixed into a basic glass component raw material solid powder, and doped with CuO, TiO2 and ZrO2. The mass ratio of the basic glass component to the doped oxides CuO, TiO2 and ZrO2 was 100:0.5:1:1.
[0053] (2) The raw material solid powder after external addition is placed in a crucible, fired at 1000°C to form glass liquid, and kept warm for 30 minutes to ensure that the glass raw material is completely melted. During this process, the heating rate is 5°C / min.
[0054] (3) Pour the glass liquid into cold water for quenching, and crush it after cooling.
[0055] (4) Pour all the glass particles into a ball mill and grind them evenly using a ball mill at a speed of 420 r / min for 2 h.
[0056] (5) Add alcohol to the coarse powder at a mass ratio of 1:1, and grind it again using a ball mill at a speed of 420 r / min for 80 min.
[0057] (6) Pour the ground alcohol-glass suspension into a tray and place it in an oven for drying. After the alcohol is completely evaporated, sieve it with a 200-mesh sieve to obtain glass powder.
[0058] (7) Glass powder, copper powder and organic carrier are mixed uniformly in a mass ratio of 4:76:20 to prepare a slurry.
[0059] (8) The slurry was coated on both ends of the ceramic body and sintered to form copper-terminal electrodes. The sintering temperature was 750°C, the temperature was kept for 15 minutes, and the heating rate was 5°C / min.
[0060] like Figures 1 to 7 As shown, the glass powder has good high-temperature wettability; after sintering, the copper terminal electrode adheres tightly to the ceramic body, the electrode surface has good density, no holes, puncture pinholes or bulging, the internal stress is moderate and evenly distributed; XRD shows glass crystallization, the crystalline phase is zinc borate (ZnB2O4), and after acid etching, the glass phase has no obvious cracks and the morphology is smooth.
[0061] Example 2
[0062] (1) B2O3, ZnO, SiO2, Al2O3, Na2O, Li2O and BaO powders are weighed in a mass percentage of 10:50:23:6:2.5:2.5:6, ground and mixed into a basic glass component raw material solid powder, and doped with CuO, TiO2 and ZrO2. The mass ratio of the basic glass component to the doped oxides CuO, TiO2 and ZrO2 is 100:1:1:1.
[0063] (2) The raw material solid powder after external addition is placed in a crucible, fired at 1000°C to form glass liquid, and kept warm for 30 minutes to ensure that the glass raw material is completely melted. During this process, the heating rate is 5°C / min.
[0064] (3) Pour the glass liquid into cold water for quenching, and crush it after cooling.
[0065] (4) Pour all the glass particles into a ball mill and grind them evenly using a ball mill at a speed of 420 r / min for 2 h.
[0066] (5) Add alcohol to the coarse powder at a mass ratio of 1:1, and grind it again using a ball mill at a speed of 420 r / min for 80 min.
[0067] (6) Pour the ground alcohol-glass suspension into a tray and place it in an oven for drying. After the alcohol is completely evaporated, sieve it with a 200-mesh sieve to obtain glass powder.
[0068] (7) Glass powder, copper powder and organic carrier are mixed uniformly in a mass ratio of 4:76:20 to prepare a slurry.
[0069] (8) The slurry was coated on both ends of the ceramic body and sintered to form copper-terminal electrodes. The sintering temperature was 750°C, the temperature was kept for 15 minutes, and the heating rate was 5°C / min.
[0070] like Figures 1 to 5 As shown, the glass powder has good high-temperature wettability; after sintering, the copper terminal electrode adheres tightly to the ceramic body, the electrode surface has good density, no holes, puncture pinholes or bulging, the internal stress is moderate and evenly distributed; XRD shows glass crystallization, the crystalline phase is zinc borate (ZnB2O4), and after acid etching, the glass phase has no obvious cracks and the morphology is smooth.
[0071] Example 3
[0072] (1) B2O3, ZnO, SiO2, Al2O3, Na2O, Li2O and BaO powders were weighed in a mass percentage of 30:40:18:4:2.5:2.5:3, ground and mixed into a basic glass component raw material solid powder, and doped with CuO, TiO2 and ZrO2. The mass ratio of the basic glass component to the doped oxides CuO, TiO2 and ZrO2 was 100:1.5:1:1.
[0073] (2) The raw material solid powder after external addition is placed in a crucible, fired at 1000°C to form glass liquid, and kept warm for 30 minutes to ensure that the glass raw material is completely melted. During this process, the heating rate is 5°C / min.
[0074] (3) Pour the glass liquid into cold water for quenching, and crush it after cooling.
[0075] (4) Pour all the glass particles into a ball mill and grind them evenly using a ball mill at a speed of 420 r / min for 2 h.
[0076] (5) Add alcohol to the coarse powder at a mass ratio of 1:1, and grind it again using a ball mill at a speed of 420 r / min for 80 min.
[0077] (6) Pour the ground alcohol-glass suspension into a tray and place it in an oven for drying. After the alcohol is completely evaporated, sieve it with a 200-mesh sieve to obtain glass powder.
[0078] (7) Glass powder, copper powder and organic carrier are mixed uniformly in a mass ratio of 4:76:20 to prepare a slurry.
[0079] (8) The slurry was coated on both ends of the ceramic body and sintered to form copper-terminal electrodes. The sintering temperature was 750°C, the temperature was kept for 15 minutes, and the heating rate was 5°C / min.
[0080] like Figures 1 to 5 As shown, the glass powder has good high-temperature wettability; after sintering, the copper terminal electrode adheres tightly to the ceramic body, the electrode surface has good density, no holes, puncture pinholes or bulging, the internal stress is moderate and evenly distributed; XRD shows glass crystallization, the crystalline phase is zinc borate (ZnB2O4), and after acid etching, the glass phase has no obvious cracks and the morphology is smooth.
[0081] Comparative Example 1
[0082] Compared with Example 1, no CuO is added to the glass powder of Comparative Example 1, and the preparation process thereof includes the following steps:
[0083] (1) B2O3, ZnO, SiO2, Al2O3, Na2O, Li2O and BaO powders were weighed in a mass percentage of 38:40:13:2:1.5:1.5:4, ground and mixed into a basic glass component raw material solid powder, and doped with TiO2 and ZrO2. The mass ratio of the basic glass component to the doped oxides TiO2 and ZrO2 was 100:1:1.
[0084] (2) The raw material solid powder after external addition is placed in a crucible, fired at 1000°C to form glass liquid, and kept warm for 30 minutes to ensure that the glass raw material is completely melted. During this process, the heating rate is 5°C / min.
[0085] (3) Pour the glass liquid into cold water for quenching, and crush it after cooling.
[0086] (4) Pour all the glass particles into a ball mill and grind them evenly using a ball mill at a speed of 420 r / min for 2 h.
[0087] (5) Add alcohol to the coarse powder at a mass ratio of 1:1, and grind it again using a ball mill at a speed of 420 r / min for 80 min.
[0088] (6) Pour the ground alcohol-glass suspension into a tray and place it in an oven for drying. After the alcohol is completely evaporated, sieve it with a 200-mesh sieve to obtain glass powder.
[0089] (7) Glass powder, copper powder and organic carrier are mixed uniformly in a mass ratio of 4:76:20 to prepare a slurry.
[0090] (8) The slurry was coated on both ends of the ceramic body and sintered to form copper-terminal electrodes. The sintering temperature was 750°C, the temperature was kept for 15 minutes, and the heating rate was 5°C / min.
[0091] like Figure 1 and 3 As shown, the glass powder has good high-temperature wettability; after sintering, the copper end electrode adheres tightly to the ceramic body, but the glass powder and copper powder do not match well, many holes appear on the end face after sintering, and after acid etching, obvious cracks appear in the glass phase and the morphology is irregular.
[0092] Comparative Example 2
[0093] Compared with Example 1, the only difference is: basic glass composition: CuO:TiO2:ZrO2=100:0.5:0:0.
[0094] Glass powder has good high-temperature wettability. After sintering, the copper end electrode will be corroded by the electroplating solution (acid) and defects will appear, and nickel leakage will occur during the later nickel plating.
[0095] Comparative Example 3
[0096] Compared with Example 1, the only difference is: basic glass composition: CuO: TiO2: ZrO2 = 100: 0.5: 1: 0.
[0097] The glass powder has good high-temperature wettability, but the amount of crystallization after sintering is low, which is not enough to optimize the overall acid resistance of the glass.
[0098] Comparative Example 4
[0099] Compared with Example 1, the only difference is: basic glass composition: CuO:TiO2:ZrO2=100:0:1:0.
[0100] The glass powder and copper powder do not match well, and the amount of crystallization after sintering is low. There are obvious traces of acid corrosion in the acid resistance test.
[0101] Comparative Example 5
[0102] Compared with Example 1, the only difference is: basic glass composition: CuO: TiO2: ZrO2 = 100: 0.5: 0: 1.
[0103] The glass powder has good high-temperature wettability, but the amount of crystallization after sintering is low, which is not enough to optimize the overall acid resistance of the glass.
[0104] In summary, the present invention synthesizes a glass powder for sintering a conductive copper paste doped with copper oxide and a nucleating agent by means of high-temperature solid-phase reaction and grinding and mixing, and then mixes the glass powder, copper powder and an organic carrier to prepare a conductive copper paste, and then coats the conductive copper paste on both ends of the ceramic body, and forms a copper terminal electrode through an integrated sintering and crystallization process. The high-temperature wetting angle of the glass powder of the present invention on a ceramic substrate such as BaTiO3 is less than 60°, which can provide a good sintering environment to reduce interference with welding wetting and welding adhesion. The glass powder of the present invention is used to prepare a microcrystalline conductive copper paste, which is used to prepare an MLCC terminal electrode. The glass powder completes the crystallization process simultaneously during the sintering and densification process with the copper powder, showing strong adhesion, high acid resistance and density with the ceramic substrate (such as BaTiO3, etc.), and the internal stress of the sintered MLCC device is moderate and evenly distributed, meeting all requirements of MLCC for the glass powder of the copper terminal electrode paste.
[0105] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A glass powder for MLCC, characterized in that: Its raw materials include: basic glass components and external components; among which, The basic glass component is boron zinc silicon system glass, and the basic glass component is composed of the following components in terms of mass percentage of oxides: B2O3 10-50%, ZnO 10-50%, SiO2 5-40%, Al2O3 1-20%, Na2O 1-10%, Li2O 1-10%, BaO 1-10%; the external doping components are CuO, TiO2 and ZrO2, and the mass ratio of the basic glass component to CuO, TiO2 and ZrO2 is 100: (0.5-1.5): (0.5-1.5): (0.5-1.5); the glass powder used for MLCC is precipitated with ZnB2O4 crystals after integrated sintering.
2. The glass powder for MLCC according to claim 1, characterized in that: The mass ratio of the basic glass component to CuO, TiO2 and ZrO2 is 100:(0.5-1.5):1:
1.
3. A method for preparing glass powder for MLCC as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: Weighing the raw materials of the basic glass component and the externally added component, grinding and mixing them into raw material solid powder; sintering the raw material solid powder into glass liquid; The glass liquid is poured into cold water for quenching, and crushed into glass particles after cooling; The glass particles are ball-milled and sieved in sequence to obtain glass powder.
4. The method for preparing glass powder for MLCC according to claim 3, characterized in that: In the process of sintering the raw material solid powder into glass liquid, the heating rate is 2-10 °C / min, the sintering temperature is 900-1200 °C, and the sintering time is 10-60 min; in the process of ball milling, a ball mill is used for ball milling, the ball mill speed is 300-600 r / min, and the ball milling time is 30-300 min; in the process of screening, the mesh size of the sieve is 200-300 mesh.
5. The method for preparing glass powder for MLCC according to claim 4, characterized in that: The ball milling includes coarse grinding and fine grinding; wherein, During the coarse grinding process, the ball milling time is 60 to 180 minutes; During the fine grinding process, alcohol needs to be added as a ball milling medium, the mass ratio of alcohol to glass powder is 1: (0.5-2), and the ball milling time is 30-120 minutes; After the fine grinding process is completed, drying treatment is required before screening to evaporate the alcohol.
6. A conductive copper paste for MLCC, characterized in that: The raw materials of the conductive copper paste for MLCC include: copper powder, organic carrier and the glass powder for MLCC as claimed in any one of claims 1 to 2.
7. The conductive copper paste for MLCC according to claim 6, characterized in that: Calculated by mass percentage, the raw materials include: 70-85% copper powder, 10-25% organic carrier, and 4-10% glass powder.
8. A multilayer ceramic capacitor, characterized in that: The multilayer ceramic capacitor comprises: a ceramic body and copper terminal electrodes, and the copper terminal electrodes are obtained by coating the conductive copper paste for MLCC as claimed in claim 6 onto both ends of the ceramic body and then subjecting the ceramic body to integrated sintering and crystallization treatment.
9. The multilayer ceramic capacitor according to claim 8, characterized in that: During the integrated sintering and crystallization process, the temperature is raised to 700-850°C at a heating rate of 1-10°C / min and kept at that temperature for 10-50 min.
Citation Information
Patent Citations
High-sintering-compactness copper paste for MLCC and preparation method of high-sintering-compactness copper paste
CN113724912A
Copper termination inks containing lead free and cadmium free glasses for capacitors
CN101238531A
Sealing microcrystalline glass, and sealing method and application thereof
CN103265176A
Method for preparing copper / ceramic composite substrate on basis of low-melting-point glass powder
CN105439643A
Electrode silver paste for functional ceramics and preparation method of electrode silver paste
CN111292873A