A high-temperature solid-phase chemical tempering method for high-Tg point glass

Through the high-temperature solid-phase chemical tempering method, solid-phase high-melting point alkali metal salts are used for ion exchange reactions, which solves the problems of long time, tedious steps and low efficiency in the existing chemical tempering methods of glass-ceramics, and realizes the LAS glass-ceramics Efficient strengthening improves bending strength and simplifies the process.

CN116535107BActive Publication Date: 2024-10-29WENZHOU KANGER CRYSTALLITE MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310573957.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-10-29
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing chemical tempering methods for glass-ceramics have problems such as complex cleaning procedures, long time-consuming steps, tedious steps, potential production safety hazards, and low efficiency. In particular, the multi-step molten salt immersion process leads to changes in the composition of the tempering agent, is time-consuming, and wastes energy. And the tempering temperature is limited by the decomposition temperature of sodium nitrate and potassium nitrate, making it impossible to achieve fast and efficient high-temperature tempering.

Method used

Adopt high-temperature solid phase chemical tempering method, use solid phase high melting point alkali metal salt as the tempering agent, set the appropriate tempering temperature and tempering agent thin layer to perform ion exchange reaction to ensure that the tempering agent does not melt, increase the ion migration rate, and achieve rapid Cooling and efficient reinforcement.

Benefits of technology

Significantly improves the bending strength of LAS glass-ceramics from 110MPa to 180MPa, simplifying the process, reducing production costs and safety risks, improving tempering efficiency, and making the tempering agent easy to clean, avoiding the complexity of multi-step processes .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535107B_ABST
    Figure CN116535107B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of deep processing of special glass, and specifically relates to a high-Tg point glass (microcrystalline glass) high-temperature solid phase chemical tempering method. The present invention comprises the following steps: setting the tempering temperature Tc of the glass to be processed; using a solid phase high melting point alkali metal salt as a tempering agent; evenly laying the tempering agent on the upper and lower surfaces of the glass to be processed to form a thin layer of the tempering agent, and the upper and lower surfaces of the glass to be processed are covered by the thin layer of the tempering agent; rapidly heating to the tempering temperature Tc of the glass to be processed and then keeping the temperature for 0.1 to 2 hours to perform ion exchange; rapidly cooling to room temperature, taking out the glass, and removing the tempering agent on its surface; and obtaining highly strengthened chemically tempered glass. The present invention can greatly improve the tempering efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of deep processing of special glass, and in particular relates to a high-temperature solid-phase chemical tempering method for high-Tg point glass (microcrystalline glass). Background Art

[0002] Glass is a common type of inorganic non-metallic material. Compared with ceramic materials, glass materials are generally weaker in strength. Glass-ceramics is a relatively unique type of glass. By adding a nucleating agent to induce nucleation, a large number of micro-nano crystals are formed inside the glass, thereby achieving reinforcement and toughening.

[0003] Lithium aluminum silicon glass-ceramic (LAS glass-ceramic) is a typical glass-ceramic. After crystallization, it has high strength and low expansion characteristics and is widely used in aerospace, kitchen appliances and other fields. The strength of common lithium aluminum silicon glass-ceramic panels can achieve 110MPa in three-point bending. When it is used in major application fields such as induction cooker panels and electric ceramic stove panels, higher strength can achieve safer application.

[0004] Glass strengthening mainly includes physical strengthening and chemical strengthening. Physical strengthening mainly involves rapid cooling after heating, which causes the glass surface to shrink rapidly and generate prestress. Chemical strengthening mainly involves surface ion exchange, replacing ions with larger radii on the glass surface with ions with smaller radii, forming higher compressive stress on the glass surface. The thermal expansion coefficient of LAS glass-ceramics is as low as 0-0.4E10 -6 , it is impossible to form prestress through rapid cooling and deformation, so the commonly used strengthening method of LAS microcrystalline glass needs to rely on chemical tempering. There are also many studies in this area.

[0005] The relevant patent reports the chemical tempering method of low expansion lithium aluminum silicon system microcrystalline glass, as follows:

[0006] 1. Patent CN 102906042A discloses a chemical tempering method for low expansion lithium aluminum silicate glass. At least two steps are used, and the strengthening agent is mainly nitrate. In the first step, the molten salt is mainly sodium nitrate, and the lithium ions on the surface of the glass are replaced by sodium ions; in the second step, the molten salt is mainly potassium nitrate, and potassium ions are further used to replace the sodium ions on the surface of the glass. For higher strength, even more tempering steps can be added. Through this method, the surface strengthening depth reaches 80 microns and the surface stress exceeds 800MPa.

[0007] 2. Patent CN110352180A discloses a chemical tempering method for low expansion lithium-containing aluminosilicate glass, which mainly uses sodium nitrate and potassium nitrate or a mixture thereof as the first tempering agent and the second tempering agent, wherein the potassium content of the second tempering agent is higher than that of the first tempering agent, and the sodium content of the second tempering agent is lower than that of the first tempering agent. The lithium-containing aluminosilicate glass is strengthened through multi-step tempering.

[0008] The above method is the mainstream strengthening method in the industry at present, which at least achieves chemical strengthening through two-step molten salt immersion. Under this system, based on a large number of experiments, it has been proved that single-step chemical strengthening, such as strengthening with pure potassium nitrate, is time-consuming and has weak effects. The two-step method or even the multi-step method can achieve relatively shorter time and improved effects. However, the above method has the following disadvantages:

[0009] 1. Cleaning process. In multi-step chemical tempering, the tempering agent composition of the previous and next processes is significantly different. When the microcrystals leave the molten salt, a lot of tempering agent is attached to the surface. If the glass is not treated and directly sent to the next tempering process, the tempering agent composition of the next process will gradually change, and the strengthening effect will be rapidly weakened. This problem is not mentioned in the above patents.

[0010] 2. It takes a long time. The first tempering step, the process of replacing Li with Na, generally takes 0.5-1.5 hours, and the second tempering step, the process of replacing Na with K, generally takes 1-6 hours. The total time of the two is 1.5-8 hours, which is also the process time mentioned in the above patent. However, after adding the cleaning step, the additional cleaning and drying steps of the glass surface tempering agent will take a lot of time.

[0011] 3. The steps are complicated. The two-step or even multi-step tempering process described in the above patents has different durations for each step. Generally, the duration of the second step is much longer than that of the first step. This will lead to a large backlog of products after the first step waiting for the second step of tempering in actual production scheduling, which can easily lead to production chaos, and the glass is repeatedly heated and cooled, wasting energy. In addition, the surface tempering agent cleaning process needs to be added, which undoubtedly puts more stringent requirements on on-site management.

[0012] 4. Production safety. In actual production, it is found that when a small amount of residual moisture on the surface of the glass directly touches the molten salt, the moisture will be instantly vaporized, resulting in a violent local explosion. If the cleaning process in the middle of the multi-step method is not dried thoroughly, a single negligence will lead to an uncontrollable production accident, which puts great pressure on safety.

[0013] 5. Low efficiency. Currently, the tempering agent mainly uses sodium nitrate and potassium nitrate, which are melted and contacted with the glass to achieve tempering. Due to the decomposition temperature of sodium nitrate and potassium nitrate, the tempering temperature cannot exceed 500°C, which greatly limits the tempering efficiency. Although some patents mention sulfates and chlorides, sodium sulfate, potassium sulfate or other salts are high melting point salts, and the melting point is generally above 700°C, which is much higher than the decomposition temperature of nitrates. Therefore, these high melting point salts cannot actually be applied to the existing molten salt immersion chemical tempering process system.

[0014] In order to address the above problems, it is urgent to develop a convenient, safe and effective chemical tempering process that can quickly achieve high-strength tempering and complete it in one step as much as possible. Summary of the invention

[0015] The technical problem to be solved by the present invention is to provide a high-temperature solid-phase chemical tempering method, thereby solving the problem of rapid strengthening of high-Tg point glass.

[0016] In order to solve the above technical problems, the present invention provides a high-temperature solid-phase chemical tempering method for high-Tg point glass, comprising the following steps:

[0017] 1) Set the tempering temperature Tc of the glass to be treated;

[0018] 2) Preparation of tempering agent:

[0019] Using solid phase high melting point alkali metal salt as a toughening agent;

[0020] The melting point of the solid phase high melting point alkali metal salt is greater than the tempering temperature Tc of the glass to be treated; thereby ensuring that the tempering agent does not melt during the tempering process;

[0021] 3) The upper and lower surfaces of the glass to be treated are evenly paved with the toughening agent to form a thin layer of the toughening agent, and the upper and lower surfaces of the glass to be treated are covered by the thin layer of the toughening agent;

[0022] The thickness of the toughening agent layer is at least 1 mm (generally 1 to 10 mm);

[0023] 4) Ion exchange:

[0024] Rapidly heat to the tempering temperature Tc of the glass to be treated and keep warm for 0.1 to 2 hours (preferably 0.8 to 2 hours);

[0025] 5) Rapidly cool to room temperature, take out the glass, and remove the toughening agent on its surface; thus, highly strengthened chemically toughened glass is obtained.

[0026] As an improvement of the high-temperature solid-phase chemical tempering method of high-Tg point glass of the present invention, the step 1): detecting and obtaining the Tg temperature of the glass to be treated; the temperature after the Tg temperature is reduced by 20 to 250° C. is the tempering temperature Tc of the glass to be treated.

[0027] Note: Tc temperature is lower than Tg temperature of glass, which can prevent the tempering temperature from being too high and stress relaxation; Tc temperature is lower than the melting point of the tempering agent, ensuring that the tempering agent does not melt during the ion exchange process.

[0028] As a further improvement of the high temperature solid phase chemical tempering method of high Tg point glass of the present invention, in the step 2):

[0029] The solid phase high melting point alkali metal salt is a high melting point potassium salt;

[0030] Alternatively, the solid phase high melting point alkali metal salt is composed of a high melting point sodium salt and a high melting point potassium salt; the high melting point sodium salt accounts for 0.01 to 50% by weight of the solid phase high melting point alkali metal salt;

[0031] High melting point sodium salts are sodium sulfate, sodium carbonate, and sodium chloride; high melting point potassium salts are potassium sulfate, potassium carbonate, and potassium chloride.

[0032] When the solid phase high melting point alkali metal salt is a high melting point potassium salt; the melting point of the high melting point potassium salt is greater than the tempering temperature Tc of the glass to be treated;

[0033] When the solid phase high melting point alkali metal salt consists of high melting point sodium salt and high melting point potassium salt, the melting point of the mixture of high melting point sodium salt and high melting point potassium salt is greater than the tempering temperature Tc of the glass to be treated.

[0034] As a further improvement of the high temperature solid phase chemical tempering method of high Tg point glass of the present invention, the step 3) is to alternately stack:

[0035] Firstly, a layer of tempering agent is laid in the container to form a thin layer of tempering agent, and then the glass to be treated and the thin layer of tempering agent are placed alternately;

[0036] That is, specifically: first lay a layer of tempering agent in the container to form a thin layer of tempering agent; then place a piece of glass to be treated, and then lay another layer of tempering agent to form a thin layer of tempering agent, and so on, a thin layer of tempering agent is laid on the upper surface of the top glass to be treated.

[0037] Note: Alternating stacking is beneficial to improving industrial efficiency, and different numbers of glass samples can be tempered at one time.

[0038] As a further improvement of the high-temperature solid-phase chemical tempering method of the high-Tg point glass of the present invention, after the thin layer of tempering agent is evenly laid on the upper and lower surfaces of the glass to be treated, compaction (overall compaction) is performed to ensure that the upper and lower surfaces of the glass to be treated are fully in contact with the thin layer of tempering agent.

[0039] As a further improvement of the high-temperature solid-phase chemical tempering method of the high-Tg point glass of the present invention, the glass to be treated is LAS microcrystalline glass, and the tempering temperature Tc of the LAS microcrystalline glass is set to 550-750°C (preferably 600-650°C).

[0040] As a further improvement of the high-temperature solid-phase chemical tempering method of the high-Tg point glass of the present invention, the solid-phase high-melting-point alkali metal salt (as a tempering agent) is composed of the following components by mass: 5-30% sodium sulfate, 20-60% potassium sulfate and 20-60% potassium chloride;

[0041] Alternatively, the solid phase high melting point alkali metal salt (as a toughening agent) is composed of the following components in mass content: 30-80% potassium chloride and 20-70% potassium sulfate.

[0042] As a further improvement of the high-temperature solid-phase chemical tempering method of the high-Tg point glass of the present invention, the solid-phase high-melting-point alkali metal salt (as a tempering agent) is composed of the following components by mass: 20% sodium sulfate, 40% potassium sulfate and 40% potassium chloride;

[0043] Alternatively, the solid phase high melting point alkali metal salt (as a toughening agent) is composed of the following components in mass content: 60% potassium chloride and 40% potassium sulfate.

[0044] As a further improvement of the high-temperature solid-phase chemical tempering method of the high-Tg point glass of the present invention, the heating rate of rapid heating is 20-30°C / min, and the cooling rate of rapid cooling is 20-30°C / min.

[0045] The present invention creates a new chemical tempering method, which does not use the traditional molten salt form of chemical tempering, but uses a solid phase high melting point alkali metal salt to directly contact the glass panel, and performs an ion exchange reaction at a high temperature far above 500°C. The tempering agent used in the present invention is completely made of high melting point salts, including alkali metal sulfates, chlorides, carbonates and other sodium and potassium salts with high melting points.

[0046] The present invention first sets a suitable tempering temperature (which is one of the technical key points of the present invention), and then prepares a suitable tempering agent.

[0047] The high-temperature solid-phase chemical tempering process described in the present invention can be applied to LAS glass-ceramics. LAS glass-ceramics is a polycrystalline multiphase material rich in micro-nano crystals and residual glass phases, and is used for black microcrystalline panels of induction cooker panels and electric ceramic cooker panels. The crystallinity can be higher than 85%, and the Tg point reaches 730-790°C. However, the current chemical strengthening method using sodium nitrate and potassium nitrate has a strengthening temperature of only within 500°C, and there is still a lot of room for improvement in the strengthening temperature.

[0048] The main components of the above-mentioned LAS glass-ceramics are as follows:

[0049]

[0050]

[0051] The LAS glass of the above formula undergoes the following crystallization process:

[0052] 1. Nucleation process: 700-740℃ for 10-60min;

[0053] 2. Crystal growth process: keep warm at 850-920℃ for 30-60min.

[0054] After cooling to room temperature, high Tg point LAS glass-ceramics can be obtained.

[0055] The glass transition point (Tg point) of LAS glass-ceramics is shown in Figure 1 , measured by DSC method.

[0056] In the present invention, the tempering temperature is determined based on:

[0057] 1. A certain temperature below the Tg point to avoid thermal relaxation;

[0058] 2. Slightly lower than the melting point of the mixed tempering agent to prevent the tempering agent from melting.

[0059] The basis for the design of toughening agent formula:

[0060] 1. K salt content is dominant, and the strengthening effect is good;

[0061] 2. Sodium salt can be added appropriately to lower the melting point to a reasonable range below the Tg point.

[0062] In the solid-phase high-temperature tempering process described in the present invention, the tempering agent remains in a solid state during the tempering process, which is significantly different from the current chemical tempering method. By raising the tempering temperature to close to the Tg point and increasing the ion migration rate, the potassium ions in the tempering agent can penetrate into the glass surface in the solid phase, forming a large compressive stress on the surface. The method of the present invention greatly increases the tempering temperature to 550-750°C, greatly improving the tempering efficiency. After tempering by the process described in the present invention, the surface of the LAS microcrystalline glass remains smooth, without surface damage, and the surface tempering agent is extremely easy to clean.

[0063] It should be noted that LAS glass-ceramics is only a typical application example, and the process of the present invention is applicable to various types of glass with high Tg points to which lithium or sodium elements are added.

[0064] The method of the present invention can improve the bending strength of low-expansion LAS glass-ceramics from 110 MPa to 180 MPa, and the improvement effect is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0066] Figure 1 is the glass transition point (Tg point) of the LAS glass-ceramics obtained in Example 1;

[0067] Figure 2 The three-point bending test report of Example 1;

[0068] Figure 3 This is the three-point bending test report for comparative example 1. DETAILED DESCRIPTION

[0069] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0070] Example 1: A LAS glass-ceramic (this is conventional technology):

[0071] The glass composition is as follows:

[0072] SiO2 63%,

[0073] Al2O3 19%,

[0074] Li2O 3.8%,

[0075] Na2O 0.5%,

[0076] K2O 0.5%,

[0077] MgO 1%,

[0078] CaO 0.5%,

[0079] BaO 3%,

[0080] ZnO 1.5%

[0081] TiO2 4%

[0082] ZrO22%

[0083] SnO2 0.3%

[0084] CeO2 0.7%,

[0085] Impurity content 0.2%.

[0086] The crystallization process is as follows:

[0087] ——720℃ for 20min;

[0088] ——870°C for 45 minutes.

[0089] The Tg point temperature of crystallized LAS glass-ceramics is about 790°C ( Figure 1 ). The Tc temperature can be set to be 20-250°C lower than the glass Tg temperature, so the tempering temperature Tc can be set to 550-750°C first.

[0090] The thickness of the prepared LAS microcrystalline panel is 4 mm. The three-point bending strength is measured, and the bending strength is about 110 MPa.

[0091] Ingredients used as toughening agents:

[0092] The melting point of sodium sulfate is 884°C; the melting point of potassium sulfate is 1067°C; the melting point of potassium chloride is 770°C; the melting point of sodium chloride is 801°C; the melting point of sodium carbonate is 851°C, and the melting point of potassium carbonate is 891°C. The eutectic point of the mixed salt will be lower than the melting point of the single component.

[0093] Example 1: A high-temperature solid-phase chemical tempering method for high-Tg glass (LAS glass-ceramics of Example 1), comprising the following steps:

[0094] (1) Setting the tempering temperature Tc of LAS glass-ceramics to 600°C;

[0095] (2) preparing a mixture of sodium sulfate, potassium sulfate and potassium chloride in a mass ratio of 20:40:40, and mixing the mixture evenly to obtain a tempering agent;

[0096] (3) placing a thin layer of toughening agent (the toughening agent obtained in step (2)) and the LAS microcrystalline panel obtained in Example 1 alternately;

[0097] Specifically: first lay a layer of tempering agent in the container (thereby forming a thin layer of tempering agent); then place a piece of LAS microcrystalline glass, and then lay a layer of tempering agent, and so on, a layer of tempering agent is laid on the upper surface of the LAS microcrystalline glass at the top; the thickness of the thin layer of tempering agent is about 2mm.

[0098] Alternating stacking is beneficial to improving industrial efficiency, and different numbers of glass samples can be tempered at the same time.

[0099] (4) Compaction:

[0100] After laying the last layer of toughening agent, compact the whole surface (under a pressure of 0.2-20kPa for 10-120 seconds) to ensure that the microcrystalline panel is in full contact with the thin layer of toughening agent.

[0101] (5) Rapidly increase the temperature to 600°C at a heating rate of 25°C / min and keep at this temperature for 90 minutes;

[0102] (6) Rapidly cool the glass to room temperature at a cooling rate of 30°C / min and simply scrape off the solid tempering agent on the glass surface.

[0103] The three-point bending strength of the glass-ceramic sample obtained after high-temperature solid chemical tempering treatment in step (6) was measured, and the bending strength was about 174 MPa.

[0104] Note: The three-point bending strength test method is in accordance with GB / T 37781-2019, repeated 4 times, and the average is rounded.

[0105] Embodiment 2: Compared with Embodiment 1, the following changes are made:

[0106] In step (1): setting the tempering temperature Tc of the glass to 650°C;

[0107] In step (2), the tempering agent is obtained by mixing potassium chloride and potassium sulfate in a mass ratio of 60:40;

[0108] In step (5), the temperature is rapidly raised to 650° C. and kept at this temperature for 50 minutes;

[0109] The rest is the same as Example 1.

[0110] The three-point bending strength of the glass-ceramic sample after high-temperature solid chemical tempering treatment was measured, and the bending strength was about 181Mpa.

[0111] Embodiment 3: Compared with Embodiment 1, the following changes are made:

[0112] In step (1): setting the tempering temperature Tc of the glass to 580°C;

[0113] In step (2), the toughening agent is obtained by mixing sodium carbonate, potassium carbonate and potassium chloride in a mass ratio of 10:40:50;

[0114] In step (5), the temperature is rapidly raised to 580° C. and kept at this temperature for 120 minutes;

[0115] The rest is the same as Example 1.

[0116] The three-point bending strength of the glass-ceramic sample after high-temperature solid chemical tempering treatment was measured, and the bending strength was about 149Mpa.

[0117] Comparative Example 1

[0118] (1) preparing a first tempering agent, weighing sodium nitrate and potassium nitrate in a weight ratio of 90:10, heating to 380° C. and then maintaining the temperature, so that the first tempering agent melts into a liquid state;

[0119] (2) immersing the LAS microcrystalline panel obtained in Example 1 in the tempering solution obtained in step (1), and maintaining the temperature at 380° C. for 30 minutes;

[0120] (3) The LAS microcrystalline panel that has been tempered in step 2 is taken out, cleaned, and dried, which takes 30 minutes;

[0121] (4) preparing a second tempering agent, weighing sodium nitrate and potassium nitrate in a weight ratio of 5:95, heating to 450° C. and then maintaining the temperature, so that the second tempering agent melts into a liquid state;

[0122] (5) immersing the cleaned LAS microcrystalline panel obtained in step 3 in the tempering solution obtained in step 4, and maintaining the temperature at 450° C. for 3 hours;

[0123] (6) Take out the LAS glass-ceramic panel, cool it to room temperature, and then rinse and dry it.

[0124] The three-point bending strength of the glass-ceramic sample after the secondary chemical tempering treatment obtained in step 6 was measured, and the bending strength was about 142 MPa.

[0125] The specific parameters are described in Table 2.

[0126] Table 2

[0127]

[0128]

[0129] Example 4-1: The tempering agent in Example 2 is changed to be composed entirely of potassium chloride, and the rest is the same as Example 2. The obtained result is: the bending strength is about 125 MPa.

[0130] Example 4-2: The tempering agent in Example 2 is changed to be composed entirely of potassium sulfate, and the rest is the same as Example 2. The obtained result is: the bending strength is about 120 MPa.

[0131] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. A high temperature solid phase chemical tempering method for high Tg point glass, characterized in that: The composition of LAS glass-ceramic is as follows: SiO2 63%, Al2O3 19%, Li2O 3.8%, Na2O 0.5%, K2O 0.5%, MgO 1%, CaO 0.5%, BaO 3%, ZnO 1.5%, TiO2 4%, ZrO22%, SnO2 0.3%, CeO2 0.7%, Impurity content 0.2%; Follow these steps: (1) Set the tempering temperature Tc of LAS glass-ceramics to 650°C; (2) The tempering agent is prepared by mixing potassium chloride and potassium sulfate in a mass ratio of 60:40; (3) placing the tempering agent and LAS microcrystalline panels alternately; The thickness of the tempering agent is 2mm, and the thickness of the LAS microcrystalline panel is 4mm; (4) Compaction: After applying the last layer of tempering agent, maintain the pressure of 0.2-20kPa for 10-120 seconds to compact the whole surface and make the microcrystalline panel fully contact with the tempering agent; (5) Rapidly increase the temperature to 650°C at a heating rate of 25°C / min and keep at this temperature for 50 minutes; (6) Rapidly cool the glass to room temperature at a cooling rate of 30°C / min and scrape off the solid tempering agent on the glass surface.

2. A high temperature solid phase chemical tempering method for high Tg point glass, characterized in that: The composition of LAS glass-ceramics is as follows: SiO2 63%, Al2O3 19%, Li2O 3.8%, Na2O 0.5%, K2O 0.5%, MgO 1%, CaO 0.5%, BaO 3%, ZnO 1.5%, TiO2 4%, ZrO22%, SnO2 0.3%, CeO2 0.7%, Impurity content 0.2%; Follow these steps: (1) Setting the tempering temperature Tc of LAS glass-ceramics to 600°C; (2) preparing a mixture of sodium sulfate, potassium sulfate and potassium chloride in a mass ratio of 20:40:40, and mixing the mixture evenly to obtain a tempering agent; (3) placing thin layers of toughening agent and LAS microcrystalline panels alternately; A layer of tempering agent is laid on the upper surface of the LAS microcrystalline glass at the top; the thickness of the tempering agent thin layer is 2mm, and the thickness of the LAS microcrystalline panel is 4mm; (4) Compaction: After applying the last layer of toughening agent, keep the pressure at 0.2-20kPa for 10-120 seconds to compact the whole surface and make sure the microcrystalline panel is in full contact with the thin layer of toughening agent. (5) Rapidly increase the temperature to 600°C at a heating rate of 25°C / min and keep at this temperature for 90 minutes; (6) Rapidly cool the glass to room temperature at a cooling rate of 30°C / min and simply scrape off the solid tempering agent on the glass surface.

Citation Information

Patent Citations

  • Chemically tempered glass

    CN102906042A

  • Lithium containing aluminosilicate glass with low expansion after chemical toughening

    CN110352180A

  • Process for ion exchange on glass or glass ceramic

    US5127931A