Method for collaboratively treating carbon-containing coal gangue and steel slag

By synergistically treating carbon-containing coal gangue and steel slag, the fixed carbon in coal gangue is used to reduce iron oxide in steel slag, the hydration activity of coal gangue and steel slag is improved, and the problem of limited amount of cement concrete is solved. ,实现了大规模利用和经济效益的提升。

CN116535148BActive Publication Date: 2024-11-15XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310507051.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-15
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

In the prior art, the utilization of coal gangue and steel slag in cemented materials is limited. Due to the low mineral hydration activity and high inert mineral content, their dosage in cement concrete is limited, making it difficult to achieve large-scale utilization.

Method used

By mixing carbon-containing coal gangue with steel slag, calcining and cooling, using the fixed carbon in the coal gangue to reduce the iron oxide in the steel slag, reducing the inert mineral content, and improving the hydration activity of coal gangue through high-temperature treatment, thereby improving its in-cement The amount of admixture in concrete.

Benefits of technology

The waste is used to make waste, which increases the amount of cement concrete and economic benefits, reduces the amount of cement water consumption, improves hydration activity, and increases the utilization value of steel slag and coal gangue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535148B_ABST
    Figure CN116535148B_ABST
Patent Text Reader

Abstract

A method for synergistically processing carbon-containing coal gangue and steel slag, wherein the carbon-containing coal gangue and steel slag are mixed to obtain a mixture, calcined at 1200-1550°C for 0.5-3h, cooled, dried, and separated to obtain metallic iron and residue. The residue is ground and can be used as a cement admixture. The present invention reduces the iron oxide in the steel slag to elemental iron, which can reduce the content of inert minerals in the residue, and rapidly cools the residual molten slag liquid to increase the hydration activity of the residue, thereby increasing its dosage in the cementitious material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mining solid waste treatment and concrete cementitious materials, and in particular relates to a method for collaboratively treating carbon-containing coal gangue and steel slag. Background Art

[0002] A large amount of coal gangue is stripped off during coal mining. These coal gangues have complex chemical compositions and multiple mineral compositions, and are difficult to utilize. They have become a major problem affecting the clean production of coal enterprises. In the prior art, the main field of comprehensive utilization of coal gangue is building materials, which can be used as road materials, cementitious materials, mine filling materials, etc. However, due to the low hydration activity of minerals in coal gangue, the residual carbon affects the water consumption of cement and reduces the strength of cementitious materials. Therefore, the amount of carbon-containing coal gangue added to cementitious materials is limited, and it is difficult to use it in large amounts.

[0003] On the other hand, the potential large-scale utilization of steel slag is also in the field of building materials. However, the high content of free calcium oxide and inert minerals in steel slag, especially the iron oxide exceeding 20%, also affects its large-scale use in cement. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for the coordinated treatment of carbon-containing coal gangue and steel slag, thereby reducing the iron oxide in the steel slag to elemental iron to reduce the content of inert minerals in the residue, and at the same time rapidly cooling the residual molten slag liquid to increase the hydration activity of the residue, thereby increasing its dosage in the cementitious material.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for collaboratively processing carbon-containing coal gangue and steel slag comprises the following steps:

[0007] Step 1, mixing carbon-containing coal gangue with steel slag to obtain a mixture;

[0008] Step 2, calcining the mixture at 1200-1550° C. for 0.5-3 h;

[0009] Step 3, cooling the calcined mixture;

[0010] Step 4, drying the cooled mixture to separate metallic iron and residue.

[0011] In one embodiment, the iron oxide content in the steel slag is greater than 35% by weight, and the carbon-containing coal gangue contains 5-30% fixed carbon.

[0012] In one embodiment, the steel slag is converter steel slag produced by steelmaking, and its chemical composition by weight is: 30-50% CaO, 10-16% SiO2, 0.5-5% Al2O3, 10-32% Fe2O3, 1-5% FeO, 1-5% Fe4O3, 0.2-8% MgO and the remainder impurities.

[0013] In one embodiment, the weight ratio range of steel slag to coal gangue is calculated according to the following chemical formula based on the carbon content in coal gangue and the Fe2O3, Fe4O3 and FeO content in steel slag:

[0014] 3C+2Fe2O3=4Fe+3CO2

[0015] 2C+Fe3O4=3Fe+2CO2

[0016] C+2FeO=2Fe+CO2

[0017] In one embodiment, in step 1, the carbon-containing coal gangue and steel slag are mixed and then crushed and ground, or crushed and ground and then mixed, or crushed and ground and then laid layer by layer.

[0018] In one embodiment, in step 2, the heating rate is 1-20° C. / min, and the heating and calcining are performed in an air atmosphere or a nitrogen atmosphere.

[0019] In one embodiment, in step 3, the cooling method is water cooling, air cooling or natural cooling. Water cooling or air cooling is preferably used.

[0020] In one embodiment, in step 4, the mixed material is dried and crushed, and the metallic iron and water-quenched slag are separated by magnetic separation.

[0021] In one embodiment, the residue is ground and used as a cement mixing material.

[0022] In one embodiment, the residue is used in a cement mixed material in an amount of 10%-70%, and the remaining component is cement.

[0023] The principle of the present invention is to use the fixed carbon in the carbon-containing coal gangue as a reducing agent to reduce the iron oxide in the steel slag, while removing a large amount of carbon. In addition, after high-temperature treatment, the carbon-containing coal gangue is thermally activated, and its hydration activity is improved, so that the amount of coal gangue added in concrete can be greatly increased.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) The purpose of using waste to treat waste is achieved by taking advantage of the inherent shortcomings of two types of solid waste that are very difficult to comprehensively utilize. The carbon in carbon-containing coal gangue leads to an increase in the water consumption of cement concrete, and the low mineral hydration activity of coal gangue itself is an important factor restricting its application in cement concrete. The iron oxide content in steel slag is high and its hydration activity is poor, and its dosage in cement concrete is also very low. The residual carbon in coal gangue is used to reduce the iron oxide in steel slag and reduce the content of inert minerals in steel slag. The melting process can also promote aluminosilicates to absorb free calcium oxide in steel slag. On the other hand, coal gangue is activated by heat, which increases the hydration activity of coal gangue and increases the dosage of coal gangue in cement concrete. In summary, the present invention achieves the effect of using waste to treat waste.

[0026] 2) Good economic efficiency. According to the current experimental results, steel slag with a Fe2O3 content of 30% can reduce about 10% of the total amount of elemental iron in steel slag and coal gangue (about 20% of the mass of steel slag). According to the current price of iron ore with an iron grade of 62% exceeding 850 yuan / ton and the price of scrap steel at 2,800 yuan / ton, the economic benefit of processing 1 ton of steel slag and coal gangue mixture alone is about 85-280 yuan, about 180 yuan on average. The cost used in the present invention is mainly the energy cost required to heat the mixture. According to the cost of 1 ton of cement being about 180 yuan, plus the economic benefit of using the residue as a cement mixing material, the present invention has good economic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the phase composition of steel slag in an embodiment of the present invention.

[0028] Figure 2 Schematic diagram of the phase composition of coal gangue in an embodiment of the present invention.

[0029] Figure 3 The present invention is a flowchart of the coordinated processing of carbon-containing coal gangue and steel slag in an embodiment of the present invention.

[0030] Figure 4 These are photos of the crucible cross-section, water-quenched slag and iron particles after the sample was cooled after reduction at 1400℃ for 30 minutes.

[0031] Figure 5 These are photos of the slag, iron particles and water-quenched slag in the crucible after the sample was cooled after reduction at 1450℃ for 30 minutes.

[0032] Figure 6 The XRD diagram of water-quenched slag obtained by keeping the mixture at 1300℃ for different time.

[0033] Figure 7 XRD patterns of water-quenched slag of samples kept at different reduction temperatures for 30 minutes.

[0034] Figure 8Hydration exothermic curves of baseline cement, cement mixed with 30% slag powder, and cement mixed with 30% water-quenched residual slag treated at 1350℃ and 1400℃.

[0035] Fig. 9 Backscattered microscopic image and element distribution map of the water-quenched residue after treatment at 1350℃.

[0036] Fig.10 Backscattered microscopic image and element distribution map of the water-quenched residue after treatment at 1400℃. DETAILED DESCRIPTION

[0037] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0038] The present invention relates to a method for collaboratively treating carbon-containing coal gangue and steel slag, wherein the content of iron oxide in the steel slag is above 35%. The present invention selects converter steel slag produced by steelmaking, and the chemical composition thereof is, by weight, 30-50% of CaO, 10-16% of SiO2, 0.5-5% of Al2O3, 10-32% of Fe2O3, 1-5% of FeO, 1-5% of Fe4O3, 0.2-8% of MgO and the remainder of impurities.

[0039] In the embodiment of the present invention, the steel slag is selected as converter slag produced by Shaanxi Longmen Iron and Steel (Group) Co., Ltd., which is subjected to heat stewing and magnetic separation treatment.

[0040] The chemical composition of the steel slag mainly includes CaO, SiO2, Al2O3, Fe2O3 and MgO. Compared with cement clinker, the CaO content of steel slag is low and the Fe2O3 and MgO content is high; compared with blast furnace slag, the SiO2 and Al2O3 content of steel slag is low and the Fe2O3 content is high. According to the general classification method, the four types of steel slag are all classified as high-basicity tricalcium silicate slag. The chemical composition of the steel slag is shown in Table 1.

[0041] Table 1 Chemical composition of steel slag wt%

[0042] CaO <![CDATA[Fe2O3]]> <![CDATA[SiO2]]> MgO <![CDATA[A12O3]]> MnO <![CDATA[P2O5]]> <![CDATA[TiO2]]> <![CDATA[V2O5]]> <![CDATA[SO3]]> <![CDATA[Na2O]]> <![CDATA[Cr2O3]]> Impurities 37.93 20.33 17.22 9.11 5.14 4.5 2.65 1.32 0.545 0.336 0.312 0.225 0.382

[0043] Figure 1 The figure is the X-ray diffraction diagram of the raw steel slag in the embodiment of the present invention. The main minerals in the steel slag include chernozemite, ferromagnesian oxide, magnetite, dicalcium silicate, periclase and leuconostocite.

[0044] Carbon-containing coal gangue is a black-gray waste rock discharged during the raw coal mining process, and the discharge amount is about 15-20% of the raw coal output. Its composition generally contains 5-30% fixed carbon. The chemical composition is mainly SiO2 and Al2O3, which has a reducing effect and a component regulating effect. In the embodiment of the present invention, its fixed carbon content is 16.84%. The chemical composition is shown in Table 2.

[0045] Table 2 Chemical composition of carbon-containing coal gangue wt%

[0046] <![CDATA[SiO2]]> <![CDATA[A12O3]]> CaO <![CDATA[Fe2O3]]> <![CDATA[K2O]]> <![CDATA[TiO2]]> <![CDATA[SO3]]> MgO <![CDATA[Na2O]]> Cl Impurities 54.64 22.99 8.17 6.08 2.65 1.78 1.54 1.01 0.42 0.12 0.60

[0047] Figure 2 This is an X-ray diffraction diagram of carbon-containing coal gangue in an embodiment of the present invention. The main minerals in the diagram are kaolin and quartz.

[0048] The fixed carbon content of carbon-containing coal gangue is calculated in accordance with GB / T 212-2008 "Industrial Analysis Methods for Coal". The industrial analysis data are shown in Table 3.

[0049] Table 3 Industrial analysis of carbon-containing coal gangue wt%

[0050] <![CDATA[M ad ]]> <![CDATA[A ad ]]> <![CDATA[V ad ]]> <![CDATA[FC ad ]]> 1.69 60.70 20.77 16.84

[0051] Where: M ad is the mass fraction of moisture in the coal sample for general analysis and testing, A ad is the mass fraction of ash on air-dry basis, V ad ——Mass fraction of volatile matter on air-dry basis, FC ad is the mass fraction of fixed carbon on an air-dried basis.

[0052] refer to Figure 3 , the method of the present invention can be described as follows:

[0053] Step 1: Mix carbon-containing coal gangue and steel slag to obtain a mixture.

[0054] Step 11: Crushing and grinding.

[0055] Specifically, steel slag and carbon-containing coal gangue were crushed into d max <8mm, then use Φ500mm×500mm test ball mill for grinding. The ball-to-material ratio of the ball mill can be 20:1, the mass of the sample ground each time shall not exceed 5kg, and the powder shall be ground to an average particle size of less than 80 microns.

[0056] Step 12, mixing the raw materials.

[0057] The steel slag and coal gangue can be mixed in a specific ratio before grinding, or they can be ground separately and then mixed evenly. The fine coal gangue powder and steel slag powder can also be spread layer by layer in the reaction container. The present invention preferably uses the method of grinding separately and then mixing evenly.

[0058] In the present invention, the weight ratio range of steel slag to coal gangue can be calculated according to the carbon content in coal gangue and the Fe2O3, Fe4O3 and FeO content in steel slag in combination with the following chemical formula:

[0059] 3C+2Fe2O3=4Fe+3CO2

[0060] 2C+Fe3O4=3Fe+2CO2

[0061] C+2FeO=2Fe+CO2

[0062] Step 2, calcination and reduction.

[0063] The mixed material is heated to a specific temperature in any heating device such as a muffle furnace, a high temperature furnace, a fluidized bed furnace, a microwave heating furnace, etc. In this embodiment, the heating rate is selected to be 1-20°C / minute, the holding temperature is 1200-1550°C, and the calcination time is 0.5-3h. Heating and calcination can be carried out in an air atmosphere or a nitrogen atmosphere. The present invention preferably uses a nitrogen protective atmosphere.

[0064] Step 3, cool.

[0065] In order to cool the calcined mixture, water cooling, air cooling, natural cooling, etc. are used. In order to avoid oxidation of the reduced elemental iron during the cooling process and to increase the activity of the residue, water cooling is preferred.

[0066] Step 5, separation of elemental iron.

[0067] The cooled mixture is dried and crushed, and then the reduced iron particles are selected using magnetic separation or other methods, thereby separating the metallic iron and the residue.

[0068] Step 6: Grinding residue is used as cement mixing material

[0069] Grind the remaining residue after the above iron selection to a specific surface area greater than 300m 2 / kg, and then used as cement admixture. In the cement admixture, the amount of the residue can be 10%-70% by weight, and the rest is cement.

[0070] In an embodiment of the present invention, a reduction test is performed on steel slag in a microwave muffle furnace. The steel slag powder is evenly mixed with carbon-containing coal gangue and put into a corundum crucible. The sample and the crucible are placed in a microwave muffle furnace and calcined under nitrogen protection. After the insulation is completed, the crucible is immediately taken out and water quenched. The water-quenched sample is dried, the metallic iron produced by the reduction is separated, and the occurrence state of the iron element in the slag sample is tested. Table 4 is a table of the ratios of coal gangue raw materials and steel slag raw materials. In order to ensure that the iron oxides in the steel slag can be fully reduced, the amount of coal gangue is increased by 10% compared to the theoretically required amount of coal gangue.

[0071] Table 4 Ingredients

[0072]

[0073] According to the chemical composition of coal gangue and steel slag in Table 1 and Table 2, the main chemical composition of the two raw materials after batching according to the batching ratio in Table 4 is calculated and shown in Table 5.

[0074] Table 5 Theoretical chemical composition of the mixture %

[0075] CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> MgO <![CDATA[Fe2O3]]> Alkalinity R 30.63 26.40 9.52 7.12 16.83 1.05

[0076] from Figure 4 It can be seen that the raw materials in the crucible are basically melted. The sizes of the spherical iron particles range from 2 mm to 1.3 cm.

[0077] from Figure 5 As can be seen in the figure, the raw materials in the crucible are melted. The round iron particles range in size from 1 cm to 3 cm. The color of the water-quenched slag is yellow and black, and the yellow color is similar to the color of slag.

[0078] from Figure 6 It can be seen that in addition to Gehlenite and Merwinite (Ca3Mg(SiO4)2), the water-quenched slag has an obvious 2θ peak near 30 degrees. Figure 6 It shows that different time of keeping at 1300℃ has little effect on the formation of glass. Figure 1 , the diffraction peaks of iron-containing minerals in the steel slag basically disappear.

[0079] from Figure 7 It can be seen that compared with Figure 1 and Figure 6 The diffraction peak of iron-containing minerals in the residue reduced at 1400°C for 30 minutes disappears, and at the same time, the peak at 30 degrees gradually increases with the increase of reduction temperature, that is, the glass content increases.

[0080] from Figure 8 It can be seen that the second exothermic peak of the treated water-quenched residue appears earlier than that of the original sample, and is close to the appearance time and exothermic rate of the second exothermic peak of cement added with 30% slag powder, indicating that the cementitious activity of the water-quenched residue produced by the synergistic treatment of carbon-containing coal gangue and steel slag is improved.

[0081] from Fig. 9 It can be seen that there are still iron particles with a particle size of about 3-6 microns in the water-quenched residue, indicating that iron element also exists in the water-quenched residue after treatment at 1350℃.

[0082] from Fig.10 It can be seen that there are still iron particles with a particle size of about several microns to tens of microns in the water quenching residue.

[0083] Therefore, the present invention treats carbon gangue and steel slag in a coordinated manner, so that carbon-containing carbon gangue and steel slag, which were originally not widely used in the field of building materials, can be used in cement mixed materials, and the amount of the residue obtained after treatment in the cement mixed materials can reach up to 70%.

[0084] Table 6 shows the strength of cement mixed with different amounts of gangue and steel slag raw materials (the content of gangue in the mixture is 24.55%), and cement mixed with residues treated by this process. It can be seen from the table that the 7d and 28d strength ratios of the water-quenched residues treated by this technology are significantly higher than those of cement mixed with gangue and steel slag raw materials. With the addition of 70% of water-quenched residues, the 28d compressive strength of cement can still reach 38.5MPa.

[0085] Table 6 Comparison of cement strengths mixed with coal gangue and steel slag raw materials and the residue of the present invention

[0086]

Claims

1. A method for co-processing carbon-containing coal gangue and steel slag, characterized in that: The steps include: Step 1, mixing carbon-containing coal gangue with steel slag to obtain a mixture, wherein the iron oxide content in the steel slag is greater than 20% by weight, and the carbon-containing coal gangue contains 5-30% fixed carbon; based on the carbon content in the coal gangue and the Fe2O3, Fe4O3 and FeO contents in the steel slag, the weight ratio range of the steel slag and the coal gangue is calculated according to the following chemical formula, and the amount of coal gangue is increased by 10% compared with the theoretical amount of coal gangue required: 3C+2Fe2O3=4Fe+3CO2 2C+Fe3O4=3Fe+2CO2 C+2FeO=2Fe+CO2 Step 2, calcining the mixture at 1300° C. for 0.5 to 3 h; wherein the heating rate is 1 to 20° C. / min, and the heating and calcining are performed in a nitrogen atmosphere; Step 3, cooling the calcined mixture; Step 4, drying the cooled mixture to separate metallic iron and residue, grinding the residue and using it as a cement mixed material, wherein the residue accounts for 70% of the cement mixed material, and the rest is cement.

2. The method for co-processing carbon-containing coal gangue and steel slag according to claim 1, characterized in that: The steel slag is converter steel slag produced by steelmaking, and its chemical composition by weight is: 30-50% CaO, 10-16% SiO2, 0.5-5% Al2O3, 10-32% Fe2O3, 1-5% FeO, 1-5% Fe4O3, 0.2-8% MgO and the remainder impurities.

3. The method for co-processing carbon-containing coal gangue and steel slag according to claim 1, characterized in that: In the step 1, the carbon-containing coal gangue and steel slag are mixed and then crushed and ground, or crushed and ground and then mixed, or crushed and ground and then laid layer by layer.

4. The method for co-processing carbon-containing coal gangue and steel slag according to claim 1, characterized in that: In step 3, the cooling method is water cooling, air cooling or natural cooling.

5. The method for co-processing carbon-containing coal gangue and steel slag according to claim 1, characterized in that: In step 4, the mixed material is dried and crushed, and the metallic iron and water-quenched slag are separated by magnetic separation.

Citation Information

Patent Citations

  • Method for reducing, quenching and tempering molten steel slags in reducing atmosphere

    CN105110660A

  • Steel slag based mineral admixture, preparation method and application thereof

    CN108178530A

  • Method for reducing and recovering iron from steel slag and preparing auxiliary cementing material from secondary slag

    CN108658483A

  • Modified steel slag as well as preparation method and application thereof

    CN113735467A