Artificial aggregate based on waste gypsum and metal tailings and preparation method thereof

By pouring waste gypsum, metal tailings and cement in a layered grid mold, the environmental pollution problem of waste gypsum and metal tailings treatment is solved, efficient utilization of resources and improvement of aggregate strength are achieved, simplifying It improves the process and reduces the cost, and is suitable for concrete projects.

CN116553851BActive Publication Date: 2024-10-25WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310466988.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-25
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively process the large amounts of waste gypsum and metal tailings produced by industrial production, resulting in environmental pollution and resource waste. Moreover, the traditional recycled aggregate preparation process is complex and costly, making it difficult to popularize.

Method used

The combined raw materials of waste gypsum, metal tailings and cement are used to form aggregate particles that meet national standards through preliminary mixing, adding dispersant and pouring in a layered grid mold for demoulding and curing, and are connected by the gelling effect of cement. particles, simplifying the process and reducing costs.

Benefits of technology

It achieves effective resource utilization of waste gypsum and metal tailings, improves the strength and fluidity of aggregates, reduces raw material costs, has a simple process, has important promotion value, can effectively handle large amounts of waste gypsum and tailings, and is in line with concrete Specification requirements for aggregates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116553851B_ABST
    Figure CN116553851B_ABST
Patent Text Reader

Abstract

The invention relates to artificial aggregates based on waste gypsum and metal tailings, including 60-70 parts of waste gypsum, 30-40 parts of metal tailings, 15-20 parts of cement, a water-cement ratio of 0.4-0.8, and 0.1-1.3 parts of dispersant. Preparation method: preliminarily stir and disperse waste gypsum, metal tailings and cement; pour water, continue stirring to form aggregate slurry; add dispersant to the aggregate slurry and continue stirring; pour the fluid aggregate slurry into a layered grid-shaped mold, demould and maintain, and obtain aggregates of the required particle size. The beneficial effects of the invention are: fully utilizing the advantages of high hardness and good chemical stability of metal tailings particles, compensating for the disadvantages of low hardness and poor chemical stability of waste gypsum powder, utilizing the gelling effect of cement, connecting metal tailings particles and waste gypsum powder through cement hydration reaction products to form aggregate particles that meet the specifications, and realizing the resource utilization of waste gypsum and metal tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering materials, and in particular to an artificial aggregate based on waste gypsum and metal tailings and a preparation method thereof. Background Art

[0002] Industrial production generates a large amount of waste gypsum. Waste gypsum is an industrial waste residue mainly composed of calcium sulfate. It is in powder form, 80% of which is calcium sulfate, as well as silicon, aluminum, iron and other components. If it is not used scientifically and reasonably, it will occupy large tracts of land resources and cause certain damage to soil and water resources.

[0003] The mining of metal mines produces a large amount of metal tailings, many of which are dumped into tailings ponds or dams. The storage not only occupies land and generates dust, but also poses a geological safety hazard. In addition, due to the limitations of technological level, these tailings have not been fully utilized.

[0004] Aggregates are the largest, indispensable and irreplaceable basic materials used in the construction of infrastructure projects such as buildings, roads and bridges. However, aggregates are non-renewable resources, and my country's industrial production and metal mining produce a large amount of waste gypsum and metal tailings in the long-term production process. Using these resources to completely or partially replace aggregates and obtain artificial aggregates based on waste gypsum and metal tailings that meet the requirements of recycled aggregate concrete is of great significance for the reuse of waste resources.

[0005] Patent CN114956628A discloses a high-strength phosphogypsum-based recycled aggregate and a preparation method thereof. The mixture is prepared by mixing phosphogypsum, slag powder, cement clinker, steel slag powder, fly ash, silica ash, and pile slurry, and then adding water to form a mixture, which is added into a ring die granulator, and is pressed into shape by a ring die and a pressure roller, and then carbonization curing and natural curing are performed. The process has complex raw materials and high production costs, which is not conducive to promotion.

[0006] Patent CN115611539A discloses a recycled aggregate and roadbed material prepared by steel slag and phosphogypsum and a preparation method thereof. The entire process flow includes: 1) grinding the steel slag and screening it into steel slag powder and steel slag particles; 2) preparing a mixture of steel slag powder, phosphogypsum and slag, stirring the mixture with admixtures in a certain ratio, and then entering an ultrafine grinding system to grind the mixture to a specific surface area of ​​not less than 450m~2 / kg to prepare a roadbed binder; 3) mixing heavy metal-contaminated viscous, sandy soil or tailings with the roadbed binder, adding water and stirring evenly, and producing the recycled aggregate through a disc granulator.

[0007] Patent CN115677306A discloses a green artificial aggregate based on phosphogypsum and a preparation method thereof, which uses phosphogypsum and waste incineration ash as main raw materials. The entire process flow includes: drying the waste incineration ash, mixing cement and phosphogypsum, pouring the dried waste incineration ash into a granulator, spraying water into the granulator, and then sprinkling the mixed powder into the granulator, continuing to spray water and sprinkle the mixed powder until the particle size of the agglomerated particles reaches 4.75 mm or more, thereby obtaining the green artificial aggregate containing phosphogypsum.

[0008] In general, the preparation of artificial aggregates basically requires the use of a granulator. The process consumes high power and has certain technical requirements for operation and use. The raw materials also require a low moisture content, which is not conducive to the promotion and application of artificial aggregates made from waste gypsum. Summary of the invention

[0009] The technical problem to be solved by the present invention is to provide an artificial aggregate based on waste gypsum and metal tailings and a preparation method to broaden the scope of comprehensive utilization of waste gypsum and metal tailings in order to address the environmental pollution problem caused by the difficulty in handling a large amount of waste gypsum generated by existing industrial production and a large amount of tailings formed by metal mining.

[0010] The technical solution of the present invention to solve the above technical problems is as follows: an artificial aggregate based on waste gypsum and metal tailings, the raw material components and their mass percentages are:

[0011] Waste gypsum: 60-70 parts, metal tailings: 30-40 parts, cement: 15-20 parts, and the water-cement ratio is 0.4-0.8, dispersant: 0.1-1.3 parts.

[0012] Based on the above technical solution, the present invention can also be improved as follows.

[0013] Furthermore, the waste gypsum is phosphogypsum or desulfurized gypsum.

[0014] Furthermore, phosphogypsum is derived from solid waste generated in the wet phosphoric acid process, has a particle size of 5μm to 50μm, a crystal water content of 20% to 25%, is mainly composed of calcium sulfate dihydrate, and also contains a small amount of impurities.

[0015] Furthermore, desulfurized gypsum is derived from the by-product of the FGD process, and has a CaSO4〃2H2O content of ≥90%, a particle size of 30μm to 100μm, and a free water content of 10%-17%.

[0016] Further, the metal tailings are iron ore.

[0017] Furthermore, iron ore sand is the remaining waste residue after the iron concentrate is selected from iron ore, and its mineral components are gangue minerals.

[0018] Furthermore, gangue minerals include: quartz, pyroxene, feldspar, garnet, amphibole and their altered minerals.

[0019] Furthermore, the cement is slag silicate cement.

[0020] Based on the above technical solution, the present invention also provides a method for preparing artificial aggregate based on waste gypsum and metal tailings, and the specific steps are as follows:

[0021] S01, preliminarily stirring and dispersing waste gypsum, metal tailings and cement;

[0022] S02, pouring water and continuing to stir to form aggregate slurry;

[0023] S03, adding a dispersant to the aggregate slurry and continuing to stir to form a fluid aggregate slurry;

[0024] S04. Pour the fluid aggregate slurry into a layered grid-shaped mold, demould, and cure to obtain aggregate of the desired particle size.

[0025] The beneficial effects of the present invention are:

[0026] 1) The chemical properties of waste gypsum are unstable, and the solid particles formed by chemical reactions have low hardness, while the metal tailings particles have high hardness and stable chemical properties. Cement, as a cementitious material, is fully and evenly mixed with water, waste gypsum and metal tailings. Dispersants are then used to improve the fluidity of the mixture formed by waste gypsum, metal tailings, cement and water. When the fluidity reaches the casting requirement, the mixture is cast into a layered grid-shaped mold, demolded and cured to meet the index requirements for concrete aggregates in the national standard "Sand, Gravel and Crushed Stone for Construction" (CBT14685-2011);

[0027] The invention makes full use of the advantages of large hardness and good chemical stability of metal tailing particles, makes up for the disadvantages of low hardness and poor chemical stability of waste gypsum powder, utilizes the gelling effect of cement, connects metal tailing particles and waste gypsum powder through cement hydration reaction products to form aggregate particles that meet the specifications, not only realizes the resource utilization of phosphogypsum and metal tailings, but also saves raw material costs and is more environmentally friendly;

[0028] 2) The aggregate of the present invention not only has a greatly improved strength compared to traditional aggregates, but also can be produced into aggregates of different particle sizes through a layered grid-shaped mold;

[0029] 3) Compared with the traditional waste gypsum comprehensive utilization method and metal tailings treatment method, the aggregate production process provided by this method is simple, low-cost, does not require traditional granulation machinery, and can consume a large amount of waste gypsum generated by industrial production and a large amount of tailings generated by metal mining, and has important promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is an exploded view of the layered grid-shaped mold described in the present invention. DETAILED DESCRIPTION

[0031] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0032] The raw material components and their mass percentages of artificial aggregates based on waste gypsum and metal tailings are:

[0033] Waste gypsum: 60-70 parts, metal tailings: 30-40 parts, cement: 15-20 parts, and the water-cement ratio is 0.4-0.8, dispersant: 0.1-1.3 parts.

[0034] Furthermore: the waste gypsum is phosphogypsum or desulfurized gypsum;

[0035] Phosphogypsum is derived from solid waste generated in the wet phosphoric acid process. Its particle size is 5μm to 50μm, and its crystal water content is 20% to 25%. It is mainly composed of calcium sulfate dihydrate, and also contains a small amount of phosphorus, fluorine, organic matter, oxides, and a small amount of heavy metals and radioactive substances.

[0036] Desulfurized gypsum is a by-product of the FGD process, with a CaSO4〃2H2O content of ≥90%, a particle size of 30μm to 100μm, and a free water content of 10%.

[0037] Metal tailings are iron ore sand, a composite mineral raw material, which is the remaining waste slag after the iron ore is selected from the iron concentrate. In addition to a small amount of metal components, its main mineral components are gangue minerals, and gangue minerals include: quartz, pyroxene, feldspar, garnet, amphibole and its altered minerals;

[0038] The cement is slag silicate cement, and the dispersant is the product described in the patent application number: 2022108256858.

[0039] In this embodiment, 12 groups of embodiments are set, see Table 1 for details:

[0040] Table 1 Example

[0041]

[0042]

[0043] The structural diagram of the layered grid mold used is shown in Figure 1The layered grid-shaped mold includes: an outer baffle 1, which includes five pieces: front, rear, left, right and bottom, which are assembled into an uncovered cube. The grid tray 2 is assembled from transverse partitions 3 and longitudinal partitions 5 through open slots 4. The assembled grid tray 2 is placed in the uncovered cube. After each layer of fluid aggregate slurry is poured, an internal flat plate 6 is placed, and then the process is repeated until the uncovered cube is filled. The top of the uncovered cube is sealed with the outer baffle 1, and the transverse partitions 3 and longitudinal partitions 5 with appropriate opening slot distances are selected according to the required aggregate size.

[0044] Slump is used to reflect the fluidity of material slurry. The measurement method is: use a trumpet-shaped slump bucket with an upper opening of 100mm, a lower opening of 200mm and a height of 300mm, fill it with aggregate slurry and fill it in three times. After each filling, use a tamping hammer to hit the bucket wall evenly from the outside to the inside 25 times. After tamping, smooth it; then pull up the bucket, the aggregate slurry will collapse due to its own weight. The height of the bucket (300mm) minus the height of the highest point of the aggregate slurry after collapse is called the slump.

[0045] The unconfined compressive strength is used to represent the solidification strength of artificial aggregates of waste gypsum and metal tailings. The determination method is: select a cubic test mold with a size of 70.5mm×70.5mm×70.5mm, cast the test mold with fluidized solidifying soil, demould after 48 hours, put it in a standard curing room with a temperature of 20±2℃ and a relative humidity>95% for curing for 28 days, and use an unconfined uniaxial press to test the compressive strength of the specimen.

[0046] The crushing index, firmness and organic matter are used as comprehensive performance indicators to test whether the recycled aggregate meets the standards. The determination method is:

[0047] The crushing index is the ratio of the weight of crushed debris to the total weight of the sample measured by the prescribed test method, expressed as a percentage. The method is as follows: a certain mass of 9.5-13.2 mm stone in an air-dried state is loaded into a cylinder of a certain specification, a simple load of 400,000 N is applied on a press for 10 minutes, static pressure is applied for 5 seconds, and the sample mass is weighed after unloading, and the crushed fine particles are screened out with a sieve with an aperture of 2.36 mm, and the sieve residue of the sample is weighed, and the crushing index can be obtained by calculation;

[0048] The crushing value, firmness value and organic matter content of recycled aggregates are determined according to the national standard "Sand and Crushed Stone for Construction" (CBT14685-2011), as shown in Table 2:

[0049] Table 2 Comprehensive performance indicators of recycled aggregate

[0050]

[0051] The crushing index, firmness and organic matter of the artificial aggregates of Examples 1 to 12 in Table 1 were used as comprehensive performance indicators to check whether they met the standards. The measured data are shown in Table 3:

[0052]

[0053]

[0054] It can be seen from Table 3 that the crushing index, firmness and organic matter content of artificial aggregates all meet the standards, that is, the comprehensive performance of artificial aggregates is good. Among them, Example 4 contains 50% waste gypsum, 33% metal tailings, 17% cement, and a water-cement ratio of 0.7, which has the best effect.

[0055] The artificial aggregates of Examples 1 to 12 in Table 1 were tested for slump and 28d unconfined compressive strength, and the data are shown in Table 4:

[0056]

[0057]

[0058] It can be seen from Table 4 that the artificial aggregates of Examples 1 to 12 can all meet the casting requirements, and the 28d unconfined compressive strength all reaches 30 MPa, especially Example 4, which has the highest strength.

[0059] The best ratio of comprehensive performance of artificial aggregates of waste gypsum and metal tailings (Example 4) was selected to measure the mixture performance, mechanical properties and durability of recycled aggregate concrete, all of which met the requirements of the current national standard "Concrete Quality Control Standard" GB 50164. Therefore, artificial aggregates based on waste gypsum and metal tailings can replace concrete sand and gravel in engineering applications.

[0060] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. An artificial aggregate based on waste gypsum and metal tailings, characterized in that: The raw material components and their mass percentages are: Waste gypsum: 60-70 parts, metal tailings: 30-40 parts, cement: 15-20 parts, and the water-cement ratio is 0.4-0.8, dispersant: 0.1-1.3 parts, the dispersant is used to improve the fluidity of the mixture formed by waste gypsum, metal tailings, cement and water; The waste gypsum is phosphogypsum or desulfurized gypsum; The phosphogypsum is derived from solid waste generated in the wet phosphoric acid process, has a particle size of 5 μm to 50 μm, a crystal water content of 20% to 25%, and is mainly composed of calcium sulfate dihydrate and contains a small amount of impurities; The desulfurized gypsum is derived from the byproduct of the FGD process, has a CaSO4·2H2O content of ≥90%, a particle size of 30 μm to 100 μm, and a free water content of 10% to 17%; The metal tailings are iron ore; The cement is slag silicate cement.

2. The artificial aggregate based on waste gypsum and metal tailings according to claim 1, characterized in that: The iron ore sand is the remaining waste residue after the iron concentrate is selected from the iron ore, and the mineral components are gangue minerals.

3. The artificial aggregate based on waste gypsum and metal tailings according to claim 2, characterized in that: The gangue minerals include: quartz, pyroxene, feldspar, garnet, amphibole and altered minerals thereof.

4. A method for preparing artificial aggregate based on waste gypsum and metal tailings as claimed in any one of claims 1 to 3, characterized in that: The specific steps are as follows: S01, preliminarily stirring and dispersing waste gypsum, metal tailings and cement; S02, pouring water and continuing to stir to form aggregate slurry; S03, adding a dispersant to the aggregate slurry and continuing to stir to form a fluid aggregate slurry; S04. Pour the fluid aggregate slurry into a layered grid-shaped mold, demould, and cure to obtain aggregate of the desired particle size.