A retarding enhancer, retarding cement for roads and preparation method thereof

By using sludge incineration ash, steel slag powder, silicon fume and desulfurization ash, the setting time of the cement on the road base is extended, its strength and stability are improved, and the cement setting time is solved in the prior art is too short and The problem of large shrinkage achieves good construction operability and compressive strength.

CN116553852BActive Publication Date: 2024-11-01SHANGHAI CEO ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310375172.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-11-01
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

The settling time of ordinary silicate cement in existing road base materials is too fast, resulting in short construction time and large shrinkage, which is prone to reflective cracks. The price of commonly used retarders is high and the amount of added amount will reduce the strength of cement, affecting the operation of construction. sex.

Method used

The retarding reinforcement consisting of sludge incineration ash, steel slag powder, silicon fume and desulfurization ash is used to extend the settling time of cement through mixing and ball milling technology, improve the mechanical properties of cement, and form more C-S-H gels and Aft crystals. Reduce shrinkage and enhance the compressive strength of cement.

Benefits of technology

It has achieved the extension of the initial and final setting time of cement on the road base, improved the strength and stability of cement, reduced the dry shrinkage rate, avoided the occurrence of reflective cracks, and reduced the use of expansion agents, and improved the construction capability. Operative.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials, and discloses a retarding enhancer, retarding cement for roads and a preparation method thereof. The retarding enhancer comprises the following raw materials in parts by weight: 40 to 70 parts of sludge incineration ash, 10 to 20 parts of steel slag powder, 5 to 15 parts of silica ash, and 10 to 20 parts of desulfurized ash. The retarding enhancer of the present application can not only meet the time-delay requirements of the retarding cement for the road base layer, but also ensure the strength of the retarding cement for the road base layer through the synergistic effect between sludge incineration ash, steel slag powder, silica ash and desulfurized ash. In addition, it can also form calcium vanadium with micro-expansion, without the need to add an expansion agent, to make up for the defect that ordinary silicate cement is prone to micro-cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a retarding reinforcing agent, retarding cement for roads and a preparation method thereof. Background Art

[0002] With the acceleration of my country's urbanization process, the output of urban sewage sludge has increased year by year. The main methods of sludge disposal include anaerobic digestion-land utilization, drying and incineration-residue landfill or building material utilization, aerobic fermentation-land utilization, and deep dehydration-emergency landfill. Among them, sludge drying and incineration technology has become the mainstream development direction of sludge reduction disposal because of its high timeliness and can achieve the harmlessness and reduction of sludge to the greatest extent. Sludge incineration and drying can achieve about 90% sludge reduction, but it will still produce about 10% of solid waste, most of which are sludge incineration residues collected by the dust removal system. They are rarely effectively treated and are mainly landfilled. Not only does it occupy land resources, but it also has the hidden danger of damaging the ecological environment and is easy to cause secondary pollution.

[0003] In recent years, my country's road construction has developed rapidly. The base layer in the road pavement structure is a structural layer directly located under the surface layer, which mainly plays the role of bearing and diffusing load stress. The quality of the pavement base material directly affects the quality and performance of the pavement. Cement-stabilized base materials are widely used in road construction due to their high strength, good water stability, and good frost resistance. Due to the long process time of mixing, paving, and compaction in road construction, cement-stabilized base materials generally require a certain allowable delay time according to construction requirements to ensure the operability of construction. However, the ordinary silicate cement used in the commonly used road base materials sets too fast, resulting in a short allowable delay time for cement-stabilized materials, which causes difficulties in construction; secondly, ordinary silicate cement has high early strength and large shrinkage, and it is very easy to shrink when used in the road base, which in turn causes reflective cracks in the road surface and causes road pavement damage. The method of adding retarders is used to extend the retarding time of cement, thereby extending the construction time, but due to the high price of retarders and the increase in the dosage, the strength of cement will be reduced.

[0004] Therefore, there is an urgent need to develop a retarding enhancer for road base cement materials that is easy to construct, can extend the delay time of road base materials, reduce shrinkage and does not affect the strength of cement, and be used in the preparation of retarding cement to ensure the operability time during road construction. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a retarding enhancer, retarding cement for roads and a preparation method thereof, so as to solve the problems in the prior art.

[0006] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0007] One of the purposes of the present invention is to provide a retarding enhancer, comprising the following raw materials in parts by weight:

[0008]

[0009] In certain embodiments, the residue of the sewage sludge incineration ash passing through a sieve with an aperture of 45 μm is ≤30%.

[0010] In certain embodiments, based on the total weight of the sludge incineration ash, the content of P2O5 in the sludge incineration ash is 10-15 wt%. The detection method of P2O5 in the sludge incineration ash of this application is carried out with reference to "Cement Chemical Analysis Method" GB / T 176.

[0011] In certain embodiments, based on the total weight of the sludge incineration ash, the content of silicon-aluminum oxide in the sludge incineration ash is ≥ 70 wt %. The silicon-aluminum oxide includes calcium aluminosilicate, magnesium aluminosilicate, and potassium aluminosilicate.

[0012] In certain embodiments, based on the total weight of the steel slag powder, the content of calcium oxide in the steel slag powder is ≤4.0wt%. The method for detecting the content of calcium oxide in the steel slag powder of the present application is carried out with reference to "YB / T 140 Chemical Analysis Method for Steel Slag".

[0013] In certain embodiments, the specific surface area of ​​the steel slag powder is ≥350m 2 / kg, preferably ≥400m 2 / kg. The specific surface area in this application is determined in accordance with the Faber method for determination of specific surface area of ​​cement GB / T 8074.

[0014] In certain embodiments, the SiO2 content of the silica fume is ≥85wt% based on the total mass of the silica fume. The method for detecting the SiO2 content in the silica fume in this application is carried out according to the experimental method for SiO2 content in "Silica Fume for Mortar and Concrete" GB / T 27690.

[0015] In certain embodiments, the specific surface area of ​​the silica fume is ≥15m 2 / g. The specific surface area detection method of silica fume in this application is tested according to "Determination of Specific Surface Area of ​​Solid Substances by Gas Adsorption BET Method" GB / T 19587.

[0016] In some embodiments, the content of active calcium oxide in the desulfurized ash is 50% to 70% by weight based on the total mass of the desulfurized ash. The method for detecting the content of active calcium oxide in the desulfurized ash in this application is carried out in accordance with the "Determination of Active Calcium Oxide Content in Sintering Flue Gas Desulfurized Ash by Acid-Base Titration Method" YB / T 4611.

[0017] The second object of the present invention is to provide a method for preparing the retarding and enhancing agent as described above, comprising the following steps: mixing the raw materials according to parts by weight to obtain the retarding and enhancing agent.

[0018] The third object of the present invention is to provide the use of the retarding enhancer as described above as a raw material in retarding cement for roads.

[0019] In certain embodiments, the slow-setting cement for roads is slow-setting cement for road base.

[0020] A fourth object of the present invention is to provide a retarding cement for roads, comprising the retarding enhancer as described above, silicate cement clinker, slag powder and fly ash.

[0021] In certain embodiments, the following raw materials are included in parts by weight:

[0022]

[0023] Preferably, the specific surface area of ​​the slag powder is 400 to 500 m 2 / kg.

[0024] Preferably, the fly ash has a sieve residue of ≤30% on a 45 μm sieve, a moisture content of ≤1.0%, and a strength activity index of ≥70%. The detection methods for the moisture content and strength activity index of the fly ash in this application refer to the provisions of GB / T 1596 "Fly ash for cement and concrete".

[0025] A fifth object of the present invention is to provide a method for preparing the retarding cement for roads as described above, comprising the following steps:

[0026] The raw materials are mixed according to weight parts and ball-milled to obtain the slow-setting cement for roads.

[0027] In certain embodiments, the ball milling time is 20 to 30 minutes.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1) The retarding agent of the present application uses sludge incineration ash with a high phosphorus content to inhibit the hydration reaction process and achieve the retarding effect. At the same time, desulfurized ash is compounded with steel slag powder, and the weak alkalinity of desulfurized ash is used to stimulate the activity of steel slag powder. The retarding agent is added to the retarding cement for roads, and the volcanic ash effect and micro-aggregate filling effect of silica ash are used to enable it to synergistically strengthen the hydration reaction with the mineral powder in the retarding cement for roads in a highly alkaline liquid phase system, generate more CSH gel and Aft crystals, and thus improve the mechanical properties of the retarding agent.

[0030] 2) The retarded cement for roads of the present application is obtained by synergistically utilizing a retarded strengthening agent, slag, fly ash and silicate cement clinker, with an initial setting time of 310 to 382 minutes and a final setting time of 380 to 513 minutes. The retarded strengthening agent can not only meet the delay time requirements of the road base material, but also ensure the strength of the road base retarded cement. In addition, calcium vanadium with micro-expansion is formed under the synergistic effect of various solid wastes, and no additional expansion agent is needed to make up for the defect that ordinary silicate cement is prone to micro cracks, so that the 25d shrinkage rate of the retarded cement for roads is 0.032 to 0.034%.

[0031] 3) The retarding cement for roads of the present invention is obtained by grinding raw materials such as silicate clinker, slag powder, fly ash, and retarding enhancer. The raw materials are all powder materials with good grindability, and the process is simple. The uniformity of the distribution of the retarding enhancer can be further ensured by ball milling mixing, and the cement setting time can be extended and stabilized. In addition, by controlling the ball milling time to 20 to 30 minutes, the specific surface area of ​​the retarding cement of the road base is increased, the reaction area of ​​the sludge incineration ash participating in the reaction is increased, and the retarding effect of phosphorus is maximized. DETAILED DESCRIPTION

[0032] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0033] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0034] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0035] One of the purposes of the present invention is to provide a retarding enhancer, comprising the following raw materials in parts by weight:

[0036]

[0037] In some embodiments, the weight of the sludge incineration ash can be 40 to 53 parts, or 49 to 64 parts, or 58 to 70 parts, for example, 40 parts, 45 parts, 50 parts, 60 parts, 65 parts, 70 parts, or a range consisting of any two of these values. In some specific embodiments, it is 65 parts or 70 parts. Preferably, the sludge incineration ash is obtained by incinerating the sludge and then ball milling, and more preferably, the sludge comes from an urban sewage treatment plant; more preferably, the incineration temperature is 450°C to 1000°C; more preferably, the rotation speed of the ball mill is 300r / min to 500r / min, and the ball milling time is 10min to 30min.

[0038] In certain embodiments, the residue of the sewage sludge incineration ash passing through a sieve with an aperture of 45 μm is ≤30%.

[0039] In certain embodiments, based on the total weight of the sludge incineration ash, the content of P2O5 in the sludge incineration ash is 10-15 wt%. The detection method of P2O5 in the sludge incineration ash of this application is carried out with reference to "Cement Chemical Analysis Method" GB / T 176.

[0040] In some embodiments, the content of silicon aluminum oxide in the sludge incineration ash is not less than 70wt% based on the total mass of the sludge incineration ash. The silicon aluminum oxide includes calcium aluminosilicate, magnesium aluminosilicate, and potassium aluminosilicate. Below this range, the activity will decrease, resulting in a reduction in its dosage in the retarder enhancer, and the purpose of solid waste disposal cannot be achieved.

[0041] In some embodiments, the weight of the steel slag powder can be 10 to 16 parts, 14 to 18 parts, or 16 to 20 parts, for example, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, or a range consisting of any two of these values. In some specific embodiments, it is 12 parts, 18 parts, or 20 parts. Preferably, the steel slag powder is a product of converter or electric furnace steel slag that has been subjected to magnetic separation and iron removal and then ground; the specific surface area of ​​the steel slag powder is ≥350m 2 / kg, preferably ≥400m 2 / kg. The basic properties of the steel slag powder in this application shall comply with the requirements of "Steel Slag Powder for Cement and Concrete" GB / T 20491.

[0042] In certain embodiments, based on the total mass of the steel slag powder, the content of calcium oxide in the steel slag powder is ≤4.0%. The detection method of calcium oxide content in the steel slag powder of the present application is carried out with reference to "Chemical Analysis Methods for Steel Slag" YB / T 140.

[0043] In certain embodiments, the specific surface area of ​​the steel slag powder is ≥350m 2 / kg. The specific surface area in this application is determined according to the Faber method for determining specific surface area of ​​cement GB / T8074.

[0044] In some embodiments, the weight of the silica ash can be 5 to 9 parts, 8 to 12 parts, or 10 to 15 parts, for example, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, or a range consisting of any two of these values. In some specific embodiments, it is 5 parts or 8 parts. Preferably, the silica ash refers to the dust discharged through the flue during the smelting of ferroalloys or industrial silicon, and the powder material with qualitative silicon dioxide as the main component is obtained by collecting it.

[0045] In certain embodiments, based on the total mass of the silica fume, the SiO2 content of the silica fume is ≥85%.

[0046] In certain embodiments, the specific surface area of ​​the silica fume is ≥15m 2 / g. The method for determining the specific surface area in this application is in accordance with "Determination of the specific surface area of ​​solid substances by gas adsorption BET method" GB / T 19587

[0047] In some embodiments, the weight of the desulfurized ash can be 10 to 16 parts, 13 to 17 parts, or 16 to 20 parts, for example, 10 parts, 13 parts, 16 parts, 19 parts, 20 parts, or a range consisting of any two of these values. In some specific embodiments, it is 10 parts or 12 parts. Preferably, the desulfurized ash in this application refers to the desulfurized lime in the sintering flue gas and its desulfurized products, which are collectively referred to as sintering flue gas desulfurized ash.

[0048] In certain embodiments, based on the total mass of the desulfurized ash, the content of active calcium oxide in the desulfurized ash is 50% to 70 wt%.

[0049] The second object of the present invention is to provide a method for preparing the retarding and enhancing agent as described above, comprising the following steps: mixing the raw materials according to parts by weight to obtain the retarding and enhancing agent.

[0050] The third object of the present invention is to provide the use of the retarding enhancer as described above as a raw material in retarding cement for roads.

[0051] In some embodiments, the road retarding cement is a road base layer retarding cement. The road surface structure mainly includes a surface layer, a base layer and a subbase layer. The road base layer refers to the main load-bearing layer directly under the asphalt pavement layer and filled with high-quality materials, or the structural layer directly under the cement concrete surface layer and paved with high-quality materials.

[0052] A fourth object of the present invention is to provide a retarding cement for roads, comprising the retarding enhancer as described above, silicate cement clinker, slag powder and fly ash.

[0053] In certain embodiments, the following raw materials are included in parts by weight:

[0054]

[0055] Preferably, the weight of the retarder enhancer can be 10-18 parts, 17-25 parts, or 22-30 parts, for example, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, or a range consisting of any two of these values. In some specific embodiments, it is 12.5 parts, 13 parts, 17 parts, 25 parts, and 26 parts.

[0056] Preferably, the weight of the silicate cement clinker can be 65-67 parts, 66-68 parts, or 67-70 parts, for example, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts and 70 parts or a range consisting of any two of these values. In some specific embodiments, it is 65 parts, 67 parts and 70 parts. The silicate cement clinker is a hydraulic cementitious material with calcium silicate as the main mineral component, which is made of limestone and clay as the main raw materials, crushed, batched and ground into raw materials, and then calcined in a cement kiln. The silicate cement clinker is mainly composed of four oxides: CaO, SiO2, Fe2O3, and Al2O3, which account for more than 95wt% of the clinker, and less than 5wt% are other oxides, such as MgO, SO3, etc., which meet the requirements of GB-T21372 "Silica Cement Clinker".

[0057] Preferably, the weight portion of the slag powder can be 5 to 7 parts, or 6 to 8 parts, or 7 to 10 parts, for example, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts and 10 parts, or a range consisting of any two of these values. In some specific embodiments, it is 5 parts, 8 parts, 9.5 parts, and 10 parts.

[0058] Preferably, the specific surface area of ​​the slag powder is 400 to 500 m 2 / kg.

[0059] Preferably, the weight portion of the fly ash can be 3 to 8 parts, or 6 to 11 parts, or 8 to 12 parts, for example, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts and 12 parts, or a range consisting of any two of these values. In some specific embodiments, it is 3 parts, 4 parts, 5 parts, 9 parts and 11 parts.

[0060] Preferably, the fly ash has a sieve residue of ≤30% on a 45 μm sieve, a moisture content of ≤1.0%, and a strength activity index of ≥70%. The detection methods for the moisture content and strength activity index of the fly ash in this application refer to the provisions of GB / T1596 "Fly ash for cement and concrete".

[0061] A fifth object of the present invention is to provide a method for preparing the retarding cement for roads as described above, comprising the following steps:

[0062] The raw materials are mixed according to weight parts and ball-milled to obtain the slow-setting cement for roads.

[0063] In certain embodiments, the ball milling time is 20 to 30 minutes.

[0064] The present application uses ball milling to make the retarding enhancer, silicate cement clinker, slag powder and fly ash mixed more evenly on the one hand, so that the setting time of the retarding cement for roads is consistent, avoiding the problem of different setting times caused by uneven mixing; on the other hand, it increases the specific surface area of ​​the retarding cement and improves its activity.

[0065] In the following embodiments of the present application, the residue of sludge incineration ash passing through a sieve with an aperture of 45 μm is 22.3%; based on the total mass of the sludge incineration ash, the silicon aluminum oxide content of the sludge incineration is 75%, and the P2O5 content in the sludge incineration ash is 12%.

[0066] In the following examples of this application, the slag powder is blast furnace slag powder with a specific surface area of ​​400 to 500 m 2 / kg.

[0067] In the following examples of this application, the steel slag powder is electric furnace steel slag powder with a specific surface area of ​​400m 2 / kg; based on the total mass of the steel slag powder, the content of calcium oxide in the steel slag powder is ≤4.0wt%.

[0068] In the following embodiments of this application, the specific surface area of ​​silica fume is ≥15m 2 / g; based on the total mass of silica ash, the content of SiO2 in silica ash is ≥85%.

[0069] In the following embodiments of the present application, the content of active calcium oxide in the desulfurization ash is 50% to 70% based on the total mass of the desulfurization ash.

[0070] In the following examples of the present application, the fly ash has a 45 μm sieve residue of 23.6, a water content of 0.5%, and a strength activity index of ≥70%.

[0071] Examples 1-5

[0072] Referring to the formula in Table 1, sludge incineration ash, steel slag powder, silica ash and desulfurization ash are mixed to obtain a retarding enhancer; then referring to the formula in Table 2, the retarding enhancer obtained according to Table 1 is mixed with silicate cement clinker, slag powder and fly ash respectively, and ball milled for 25 minutes to obtain retarding cement for roads.

[0073] Table 1 Retarding and strengthening agent (parts by weight)

[0074] Example 1 Example 2 Example 3 Example 4 Example 5 Sludge incineration ash 65 70 65 45 55 Steel slag powder 18 12 20 20 20 Silica Fume 5 8 5 15 10 Desulfurization ash 12 10 10 20 15

[0075] Table 2 Slow-setting cement for roads (parts by weight)

[0076] Example 1 Example 2 Example 3 Example 4 Example 5 Retarder enhancer (part) 25 26 12.5 13 17 Portland cement clinker (parts) 65 65 67 70 70 Slag powder (parts) 5 5 9.5 8 10 Fly ash (parts) 5 4 11 9 3

[0077] Comparative Examples 1-7

[0078] The retarding and enhancing agents of Comparative Examples 1-7 were prepared with reference to the formula in Table 3, and the performance of the retarding and enhancing agents of Comparative Examples 1-7 and Example 5 was examined in terms of setting time, activity, etc.

[0079] Table 3 Retarding agent (parts by weight)

[0080]

[0081] Among them, - means no addition.

[0082] As can be seen from Table 3, the retarding enhancers of Comparative Examples 1-7 are used in retarding cement, and their setting time is shorter than that of Example 5, and their compressive strength is substantially lower than that of Example 5. It can be seen from this that the lack of sludge incineration ash in the retarding enhancer will shorten the setting time of the prepared retarding cement, and the lack of silica fume will reduce the strength of the retarding cement. In addition, the compounding of steel slag powder and desulfurization ash in the retarding enhancer can stimulate the activity of steel slag powder. Therefore, the retarding enhancer of the present application shortens the setting time and improves the compressive strength by coordinating and selecting the four components of sludge incineration ash, steel slag powder, silica fume and desulfurization ash.

[0083] Comparative Example 8

[0084] Comparative Example 8 is a commercially available slow-setting cement for roads, and its formula is as follows:

[0085] Table 4 Commercially available slow-setting cement formula for roads %

[0086] Portland cement clinker Industrial by-product gypsum Mineral powder Fly ash 66 4 10 20

[0087] Performance test: The performance tests of the retarded cements obtained in Examples 1-5 and the commercially available retarded cement for roads in Comparative Example 1 were carried out, including tests on specific surface area, flexural strength, compressive strength, shrinkage rate and setting time. The results are shown in Table 3.

[0088] Specific surface area test: The specific surface area is measured according to the Faber method for determination of specific surface area of ​​cement GB / T 8074.

[0089] Flexural strength and compressive strength: The flexural strength and compressive strength at the 7th and 28th day were measured in accordance with the provisions of "Slow-setting Portland Cement for Road Base" GB T 35162-2017

[0090] Shrinkage rate (expansion rate): Determine the length change rate in accordance with the provisions of "Test method for expansion rate of expansive cement" JC / T 313.

[0091] Setting time: Determine the initial setting time and final setting time in accordance with the provisions of "Water consumption, setting time and stability of quaternary ammonium salt method for cement standard consistency" GB / T13446.

[0092] Table 4 Test data of slow setting cement for roads of Examples 1-5

[0093]

[0094] As can be seen from Table 4, the various properties of the retarded cement for road base of this application meet the standard requirements, and the strength meets the strength grade of 32.5 retarded cement for road base, the compressive strength and flexural strength at 7d are not less than 15.0MPa and 3.0MPa, respectively, and the compressive strength and flexural strength at 28d are not less than 32.5MPa and 6MPa, respectively. Compared with the commercially available retarded cement for road, the retarded cement for road of this application has an initial setting time of more than 310min, a final setting time of more than 380min, a longer setting time, and is stable, with good construction operability; in addition, the shrinkage rate is 0.032% to 0.034%, which is low and not prone to cracks.

[0095] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A retarding enhancer, characterized in that: Contains the following raw materials in parts by weight: 40-70 parts of sludge incineration ash 10-20 parts of steel slag powder Silica fume 5-15 parts 10-20 parts of desulfurization ash; Based on the total mass of the sludge incineration ash, the content of P2O5 in the sludge incineration ash is 10-15wt%, and the content of silicon aluminum oxide in the sludge incineration ash is ≥70wt%; Based on the total mass of the steel slag powder, the content of calcium oxide in the steel slag powder is ≤4.0wt%; Based on the total mass of the desulfurized ash, the content of active calcium oxide in the desulfurized ash is 50% to 70%; The residue of the sludge incineration ash passing through a sieve with an aperture of 45 μm is ≤30%; the specific surface area of ​​the steel slag powder is ≥350m 2 / kg; the specific surface area of ​​the silica fume is ≥15m 2 / g.

2. The slow setting enhancer according to claim 1, characterized in that: Include at least one of the following technical features: 1) The specific surface area of ​​the steel slag powder is ≥400m 2 / kg; 2) Based on the total mass of the silica ash, the content of SiO2 in the silica ash is ≥85%.

3. The method for preparing the retarding and strengthening agent according to any one of claims 1 to 2, characterized in that: The method comprises the following steps: mixing the raw materials according to weight parts to obtain the retarding enhancer.

4. Use of the retarding enhancer according to any one of claims 1 to 2 as a raw material in retarding cement for roads.

5. A slow-setting cement for roads, characterized in that: The method comprises the retarding and enhancing agent as described in any one of claims 1 to 2.

6. The slow-setting cement for roads as claimed in claim 5, characterized in that: Contains the following raw materials in parts by weight: 10~30 parts of retarder enhancer 65-70 parts of Portland cement clinker 5-10 parts slag powder 3 to 12 parts of fly ash.

7. The slow-setting cement for roads as claimed in claim 6, characterized in that: The fly ash has a sieve residue of ≤30% passing through a 45 μm sieve, a moisture content of ≤1.0%, and a strength activity index of ≥70%.

8. The slow-setting cement for roads as claimed in claim 6, characterized in that: The specific surface area of ​​the slag powder is 400-500m 2 / kg.

9. The method for preparing slow-setting cement for roads according to any one of claims 6 to 8, characterized in that: The method comprises the following steps: mixing various raw materials according to weight parts, and ball milling to obtain the slow-setting cement for roads.

10. The preparation method according to claim 9, characterized in that: The ball milling time is 20 to 30 minutes.