A kind of regenerated wood fiber cement-based repair material and its preparation process
By using modified recycled wood fiber and pyrite magnetic tailings in cement-based repair materials, the problem of insufficient bonding ability between repair surfaces and repair materials in the existing technology is solved, significantly improving the repair effect and achieving high resource utilization. Value utilization.
Patent Information
- Application Number
- CN202310555866.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-17
AI Technical Summary
When existing cement-based repair materials are used to repair concrete prefabricated components, the bonding ability between the repair surface and the repair material is weak, resulting in poor repair effect and prone to the problem of the repair material falling off.
Using recycled wood fiber and pyrite magnetic separation tailings, through the combination of modified recycled wood fiber and pyrite magnetic separation tailings, the mechanical properties of the repair material are improved, the bonding force between the repair surface and the repair material is improved, and the pyrite is used Mineral magnetic separation tailings act as an activator to activate the repair surface, increase the hydration reaction, and form hydrated calcium sulfoaluminate to improve early strength and compactness.
Significantly improves the mechanical properties of the repair surface and the bonding force between the repair material and the repair surface, reduces the phenomenon of the repair material falling off, enhances the repair effect, and realizes the high-value resource utilization of waste wood fiber and pyrite magnetic separation tailings use.
Smart Images

Figure CN116553889B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete repair, and in particular to a regenerated wood fiber cement-based repair material and a preparation process thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Precast concrete components are an important part of prefabricated buildings and have been widely used in the fields of construction, bridges, and road construction. Precast concrete components are prefabricated in the factory in advance and then transported and transferred to the construction site for hoisting and construction. In the above process, precast concrete components are often damaged or cracked due to bumps and collisions, which not only affects the integrity and appearance of the precast components, but also affects the function of the precast components in severe cases. Therefore, it is an important task to repair precast concrete components with the above problems in a timely manner.
[0004] At present, the conventional repair method mainly uses cement-based repair materials to repair damaged, cracked and other parts. However, this method has the problem that the bonding ability between the damaged and cracked surface (i.e., the repair surface) and the repair material is weak, which easily causes problems such as the repair material falling off. One of the reasons is that the repair surface on the prefabricated component has strong water absorption, which will absorb a large amount of water from the repair material, resulting in insufficient water in the repair material at the repair surface, which in turn leads to the inability to fully hydrate the cement component in the repair material and form sufficient cementitious components, resulting in the phenomenon of interface stratification between the prefabricated component and the repair material, resulting in insufficient mechanical properties of the repair surface and poor repair effect. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a regenerated wood fiber cement-based repair material and a preparation process thereof, which utilizes pyrite magnetic separation tailings and regenerated wood fiber to not only improve the mechanical properties of the repair surface, but also contribute to the high-value resource utilization of waste wood fiber and pyrite magnetic separation tailings. Specifically, the technical solution of the present invention is as follows.
[0006] In the first aspect, the present invention provides a recycled wood fiber cement-based repair material, which comprises, by weight, 45-62 parts of cement, 93-117 parts of fine aggregate, 11-15 parts of pyrite magnetic separation tailings, 4-7.5 parts of recycled wood fiber, 25-37 parts of water, 0.9-1.4 parts of water reducer, and 0.7-1.1 parts of retarder. The pyrite magnetic separation tailings are ultrafine mineral powders associated with pyrite.
[0007] Furthermore, the regenerated wood fiber is a modified regenerated wood fiber, and its preparation process comprises the following steps:
[0008] (1) Place the regenerated wood fiber in an aqueous solution containing triethanolamine, stir evenly and let stand. 3+ Stir well and let it stand again.
[0009] (2) After the above step (1) is completed, the solid product in the reaction system is separated, washed and dried to obtain the modified regenerated wood fiber.
[0010] Furthermore, in step (1), the mass fraction of triethanolamine in the aqueous solution is 3-6%. This step utilizes the water absorption characteristics of the regenerated wood fiber to load triethanolamine onto the fiber, which is beneficial to the Al 3+ At the same time, triethanolamine also plays the role of early strength agent, which helps to improve the early strength of the repair surface.
[0011] Furthermore, in step (1), the mass volume ratio of the regenerated wood fiber and the aqueous solution is 1g:30-50ml. Optionally, the length of the regenerated wood fiber is between 200 and 350 μm. Preferably, the regenerated wood fiber is wood fiber prepared from waste wood. The present invention utilizes the wood fiber to improve the repair performance while also realizing the high-value resource utilization of waste wood materials.
[0012] Furthermore, in step (1), the aqueous solution contains Al 3+ The mass fraction of the source is 10-15%. 3+ The source includes at least one of aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum acetate, etc. In this step, the triethanolamine is used to convert Al 3+ Complexation to the surface of the regenerated wood fiber not only helps to improve the dispersibility of the regenerated wood fiber, but also helps to improve the repair effect of the repair material.
[0013] Furthermore, in step (1), the standing time is 40 to 60 minutes, and the second standing time is 30 to 45 minutes.
[0014] Furthermore, in step (2), the solid product is washed with methanol or ethanol, and then dried at 40-60° C. until the moisture content of the solid product is no more than 5%, thereby obtaining the modified regenerated wood fiber.
[0015] Furthermore, the specific surface area of the pyrite magnetic separation tailings is 500 to 800 m 2 / kg. In the present invention, the pyrite magnetic separation tailings not only serve as a filler to help improve the mechanical properties of the repair material, but also use its characteristic of containing FeS2 as an activator to activate the damaged and cracked surface / repaired surface on the prefabricated component, so that the repaired surface participates in the hydration reaction of the repair material, thereby making the prefabricated component and the repair material more firmly bonded, improving the mechanical properties of the repair position, and reducing the shedding of the repair material.
[0016] Furthermore, the water reducer includes any one of: polycarboxylate water reducer, naphthalene water reducer, aliphatic water reducer, aminosulfonate water reducer and the like.
[0017] Furthermore, the retarder includes any one of lignin sulfonate, sucrose, glucose, gluconate, boric acid and the like.
[0018] Furthermore, the fine aggregate includes any one of natural sand, artificial sand, etc. Optionally, the particle size of the fine aggregate is continuously graded between 0.5 and 1.5 mm.
[0019] In a second aspect, the present invention provides a process for preparing the regenerated wood fiber cement-based repair material, comprising the following steps:
[0020] (a) mixing the pyrite magnetic separation tailings and a portion of the water and stirring them for a period of time, and then mixing the resulting mixed solution with the cement, fine aggregate, recycled wood fiber or modified recycled wood fiber and stirring them for a period of time.
[0021] (b) Then add the water reducing agent, retarder and the remaining water and stir evenly to obtain the repair material.
[0022] Furthermore, in step (a), the pyrite magnetic separation tailings and 30-45% of the water are mixed and stirred for 10-20 minutes to obtain a mixed solution.
[0023] Furthermore, in step (a), the mixed solution is mixed with cement, fine aggregate and recycled wood fiber and stirred continuously for 5 to 10 minutes.
[0024] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0025] When using traditional cement-based concrete repair materials to repair damaged, cracked parts of precast concrete components, there are problems such as insufficient mechanical properties of the repaired surface and poor repair effects. To this end, the present invention uses pyrite magnetic tailings and recycled wood fibers to effectively improve the mechanical properties of the repaired surface. This is mainly because: the pyrite magnetic tailings are accompanied by FeS2, which acidifies after encountering water and oxygen in the repair material, converting the FeS2 into sulfate (FeS2+O2+H2O→Fe2O3+SO4 2++H + ), after these sulfate radicals act on the repair surface of the precast concrete component, they react with the cement hydration product Ca(OH)2 therein to form calcium sulfate, and these calcium sulfates further react with the calcium aluminate in the cement clinker in the repair material to form hydrated calcium sulfoaluminate, which helps to improve the early strength of the repair material and improve the bonding strength between the repair surface and the repair material. In addition, the hydrated calcium sulfoaluminate can also provide shrinkage compensation, which helps to inhibit the pores, cracks, etc. caused by shrinkage of the repair material during the hydration and hardening process. In addition, when the repair surface is a crack, the micro-expansion brought about by the formation of the hydrated calcium sulfoaluminate can also help to increase the density of the repair material in the crack and improve the bonding force between the repair material and the repair surface. In addition, the pyrite magnetic separation tailings can also be used as a filler to improve the pore structure of the repair material and improve its density, which helps to improve the bonding force between the repair material and the repair surface.
[0026] In summary, the present invention utilizes the pyrite magnetic tailings as an activator to activate the repair surface on the prefabricated component, so that it participates in the hydration reaction of the repair material, which is beneficial to eliminate the interface stratification phenomenon between the repair surface and the repair material, and makes the bond between the prefabricated component and the repair material stronger. In addition, by adding regenerated wood fibers, in the process of the repair surface undergoing hydration reaction to produce a gel phase, the mesh structure formed by the mutual mixing of the regenerated wood fibers and the gel phase can effectively improve the bonding force between the repair material and the repair surface and the strength of the repair material, thereby enhancing the repair effect. On the other hand, the regenerated wood fibers also play a role in retaining water. The water absorbed by the fibers replenishes moisture to the interface between the repair material and the repair surface after being released, thereby avoiding the problem of insufficient interface bonding caused by insufficient hydration reaction at the interface due to water absorption by the repair surface.
[0027] In addition, the present invention further modifies the regenerated wood fiber. First, the present invention utilizes the good adsorption capacity of the wood fiber to load triethanolamine on its surface, and then utilizes the complexing effect of triethanolamine to load Al on the surface of the wood fiber. 3+ After the wood fiber enters the repair material, in addition to the aforementioned functions, it also carries the triethanolamine and Al 3+ It also helps to reduce the agglomeration of the regenerated wood fibers and make them more evenly dispersed in the repair material. At the same time, the aluminum ions carried on the wood fibers can react with the cement in the repair material to form a three-dimensional mesh of hydrated calcium aluminosilicate (C-(A)-SH) gel products, which improves the mechanical strength and impermeability of the cemented body, thereby helping to improve the bonding force between the repair material and the repair surface and the strength of the repair material, and strengthening the repair effect. In addition, the triethanolamine carried on the regenerated wood fibers also acts as an early strength agent, which helps to improve the early bonding strength between the repair material and the repair surface of the repair material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0029] Figure 1 This is a cross-sectional SEM image of a test block prepared in the following Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer. In addition, unless otherwise defined, all professional and scientific terms used in the present invention have the same meaning as those familiar to those skilled in the art.
[0031] The reagents or raw materials used in the present invention can be purchased through conventional channels. If there is no special explanation, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only.
[0032] The regenerated wood fiber cement-based repair material and its preparation process of the present invention are now further described in detail in conjunction with the accompanying drawings and specific embodiments of the specification.
[0033] In the following examples, the pyrite magnetic separation tailings are from a certain ore processing enterprise, and the sulfur content (converted into SO3) is 4.02%. The pyrite magnetic separation tailings are magnetic minerals separated from pyrite by magnetic separation, and are associated with pyrite whose main component is FeS2.
[0034] Example 1
[0035] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0036] (1) Prepare the following raw material components: 50 parts by weight of 42.5 silicate cement, 102 parts by weight of river sand, 12.5 parts by weight of pyrite magnetic separation tailings powder, 6.0 parts by weight of recycled wood fiber powder, 30 parts by weight of water, 1.2 parts by weight of water reducer, and 0.8 parts by weight of sodium lignin sulfonate retarder. Among them: the pyrite magnetic separation tailings powder has a specific surface area of 600m 2 / kg of ultra-fine mineral powder. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a polycarboxylic acid water reducer with a water reduction rate of 25%. The length of the regenerated wood fiber powder is approximately distributed between 200 and 350 μm.
[0037] (2) The pyrite magnetic tailing powder and 13.5 parts by weight of the water were mixed and mechanically stirred for 18 minutes, and then the resulting mixture was mixed with the cement, river sand, and recycled wood fiber and mechanically stirred for 7 minutes. Then, the water reducer, retarder, and the remaining 16.5 parts by weight of water were added and mechanically stirred for 5 minutes to obtain a repair material.
[0038] Place 42.5 silicate cement and water in a mixer at a water-cement ratio of 0.45 and mix evenly to obtain cement slurry. Then pour the cement slurry into a mold to make a cubic test block with a length, width and height of 50 mm. After curing it at room temperature for 7 days, cut a straight line gap through the upper surface of the test block in the center of the upper surface. The gap is 3 mm wide and 10 mm deep. Then use the repair material prepared in this embodiment to fill and repair the above gap, and then cure it at room temperature for 7 days. Then the tensile bonding strength of the test block is measured to be 4.17 MPa. Using the same method, the splitting strength of the test block after repair by the repair material prepared in this embodiment is tested, and the result is 4.82 MPa. Figure 1 The cross-sectional SEM image of the test block prepared in this embodiment shows that the regenerated wood fibers and the cementitious phase are mixed with each other to form a network structure, which can effectively improve the bonding force between the repair material and the repair surface and the strength of the repair material, thereby enhancing the repair effect.
[0039] Example 2
[0040] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0041] (1) Prepare the following raw material components: 62 parts by weight of 42.5 silicate cement, 117 parts by weight of river sand, 15 parts by weight of pyrite magnetic separation tailings powder, 7.5 parts by weight of recycled wood fiber powder, 37 parts by weight of water, 1.4 parts by weight of water reducer, and 1.1 parts by weight of sodium gluconate retarder. Among them: the pyrite magnetic separation tailings powder has a specific surface area of 600m 2 / kg of ultra-fine mineral powder. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a polycarboxylic acid water reducer with a water reduction rate of 25%. The length of the regenerated wood fiber powder is approximately distributed between 200 and 350 μm.
[0042] (2) The pyrite magnetic separation tailing powder and 15 parts by weight of the water are mixed and mechanically stirred for 20 minutes, and then the resulting mixture is mixed with the cement, river sand, and recycled wood fiber and mechanically stirred for 10 minutes. Then, the water reducer, retarder, and the remaining 22 parts by weight of water are added and mechanically stirred for 5 minutes to obtain a repair material.
[0043] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 3.95 MPa and 4.67 MPa, respectively.
[0044] Example 3
[0045] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0046] (1) Prepare the following raw material components: 45 parts by weight of 42.5 silicate cement, 93 parts by weight of river sand, 11 parts by weight of pyrite magnetic separation tailings powder, 4 parts by weight of recycled wood fiber powder, 25 parts by weight of water, 0.9 parts by weight of water reducer, and 0.7 parts by weight of sucrose retarder. The pyrite magnetic separation tailings powder has a specific surface area of 800m 2 / kg of ultra-fine mineral powder. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a naphthalene-based water reducer with a water reduction rate of 30%. The length of the regenerated wood fiber powder is approximately distributed between 200 and 350 μm.
[0047] (2) The pyrite magnetic tailing powder and 7.5 parts by weight of the water are mixed and mechanically stirred for 10 minutes, and then the resulting mixture is mixed with the cement, river sand, and recycled wood fiber and mechanically stirred for 5 minutes. Then, the water reducer, retarder, and the remaining 17.5 parts by weight of water are added and mechanically stirred for 5 minutes to obtain a repair material.
[0048] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 4.36 MPa and 5.07 MPa, respectively.
[0049] Example 4
[0050] A preparation process of a regenerated wood fiber cement-based repair material is the same as the above-mentioned embodiment 1, except that: this embodiment uses modified regenerated wood fiber to replace the regenerated wood fiber in embodiment 1. The preparation process of the modified regenerated wood fiber comprises the following steps:
[0051] (i) The regenerated wood fiber of Example 1 was placed in an aqueous solution containing 3% triethanolamine by mass at a ratio of 1 g:50 ml, stirred evenly, and then allowed to stand for 40 minutes. Al2(SO4)3 was then added at a ratio of 12% by mass, stirred evenly, and then allowed to stand for 30 minutes.
[0052] (ii) After the above step (i) is completed, the solid product in the solution is filtered out, and then the solid product is washed twice with ethanol. After completion, the solid product is placed in an oven at 60° C. and dried until the moisture content is reduced to 3%, thereby obtaining the modified regenerated wood fiber.
[0053] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 4.92 MPa and 5.54 MPa, respectively.
[0054] Example 5
[0055] A preparation process of a regenerated wood fiber cement-based repair material is the same as the above-mentioned embodiment 2, except that: this embodiment uses modified regenerated wood fiber to replace the regenerated wood fiber in embodiment 2. The preparation process of the modified regenerated wood fiber includes the following steps:
[0056] (i) The regenerated wood fiber of Example 2 was placed in an aqueous solution containing 5% triethanolamine by mass at a ratio of 1 g:45 ml, stirred evenly, and then allowed to stand for 50 minutes. AlCl3 was then added at a ratio of 15% by mass, stirred evenly, and then allowed to stand for 40 minutes.
[0057] (ii) After the above step (i) is completed, the solid product in the solution is filtered out, and then the solid product is washed twice with ethanol. After completion, the solid product is placed in an oven at 50° C. and dried until the moisture content is reduced to 5%, thereby obtaining the modified regenerated wood fiber.
[0058] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 4.84 MPa and 5.33 MPa, respectively.
[0059] Example 6
[0060] A preparation process of a regenerated wood fiber cement-based repair material is the same as the above-mentioned embodiment 3, except that: this embodiment uses modified regenerated wood fiber to replace the regenerated wood fiber in embodiment 3. The preparation process of the modified regenerated wood fiber includes the following steps:
[0061] (i) The regenerated wood fiber of Example 3 was placed in an aqueous solution containing 6% triethanolamine by mass at a ratio of 1 g:30 ml, stirred evenly, and then allowed to stand for 60 minutes. Then, Al(NO3)3 was added at a ratio of 10% by mass, stirred evenly, and then allowed to stand for 45 minutes.
[0062] (ii) After the above step (i) is completed, the solid product in the solution is filtered out, and then the solid product is washed twice with ethanol. After completion, the solid product is placed in an oven at 40° C. and dried until the moisture content is reduced to 5%, thereby obtaining the modified regenerated wood fiber.
[0063] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 5.14 MPa and 5.88 MPa, respectively.
[0064] Example 7
[0065] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0066] (1) Prepare the following raw material components: 50 parts by weight of 42.5 silicate cement, 102 parts by weight of river sand, 6.0 parts by weight of recycled wood fiber powder, 30 parts by weight of water, 1.2 parts by weight of water reducer, and 0.8 parts by weight of sodium lignin sulfonate retarder. Wherein: the particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a polycarboxylate water reducer with a water reduction rate of 25%. The length of the recycled wood fiber powder is approximately distributed between 200 and 350 μm.
[0067] (2) The cement, river sand and recycled wood fiber are mixed and mechanically stirred for 7 minutes. Then, the water reducer, retarder and water are added and mechanically stirred for 5 minutes to obtain a repair material.
[0068] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 3.18 MPa and 3.73 MPa, respectively.
[0069] Example 8
[0070] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0071] (1) Prepare the following raw material components: 50 parts by weight of 42.5 silicate cement, 102 parts by weight of river sand, 12.5 parts by weight of pyrite magnetic separation tailings powder, 30 parts by weight of water, 1.2 parts by weight of water reducer, and 0.8 parts by weight of sodium lignin sulfonate retarder. The pyrite magnetic separation tailings powder has a specific surface area of 600m 2 / kg of ultra-fine mineral powder. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducing agent is a polycarboxylic acid water reducing agent with a water reducing rate of 25%.
[0072] (2) The pyrite magnetic tailing powder and 13.5 parts by weight of the water were mixed and mechanically stirred for 18 minutes, and then the resulting mixture was mixed with the cement and river sand and mechanically stirred for 7 minutes. Then, the water reducer, retarder and the remaining 16.5 parts by weight of water were added and mechanically stirred for 5 minutes to obtain a repair material.
[0073] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 2.66 MPa and 3.51 MPa, respectively.
[0074] Example 9
[0075] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0076] (1) Prepare the following raw material components: 62 parts by weight of 42.5 silicate cement, 117 parts by weight of river sand, 15 parts by weight of ultrafine mineral powder, 7.5 parts by weight of recycled wood fiber powder, 37 parts by weight of water, 1.4 parts by weight of water reducer, and 1.1 parts by weight of sodium gluconate retarder. The specific surface area of the ultrafine mineral powder is 600 m 2 / kg, its main component is silicon dioxide, and it does not contain pyrite. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a polycarboxylic acid water reducer with a water reduction rate of 25%. The length of the regenerated wood fiber powder is approximately distributed between 200 and 350 μm.
[0077] (2) The ultrafine mineral powder and 15 parts by weight of the water are mixed and mechanically stirred for 20 minutes, and then the resulting mixture is mixed with the cement, river sand, and ultrafine mineral powder and mechanically stirred for 10 minutes. Then, the water reducer, retarder, and the remaining 22 parts by weight of water are added and mechanically stirred for 5 minutes to obtain a repair material.
[0078] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 3.04 MPa and 3.32 MPa, respectively.
[0079] Example 10
[0080] A preparation process of a regenerated wood fiber cement-based repair material is the same as the above-mentioned embodiment 4, except that: the preparation process of the modified regenerated wood fiber comprises the following steps:
[0081] (i) Add the regenerated wood fiber of Example 1 to water at a ratio of 1 g:50 ml, stir evenly and let stand for 40 minutes. Then add Al2(SO4)3 at a mass fraction of 12%, stir evenly and let stand for 30 minutes.
[0082] (ii) After the above step (i) is completed, the solid product in the solution is filtered out, and then the solid product is washed twice with ethanol. After completion, the solid product is placed in an oven at 60° C. and dried until the moisture content is reduced to 3%, thereby obtaining the modified regenerated wood fiber.
[0083] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 4.03 MPa and 4.58 MPa, respectively.
[0084] Embodiment 11
[0085] A preparation process of a regenerated wood fiber cement-based repair material is the same as the above-mentioned embodiment 4, except that: the preparation process of the modified regenerated wood fiber comprises the following steps:
[0086] (i) The regenerated wood fiber of Example 2 was placed in an aqueous solution containing 5% by mass of triethanolamine at a ratio of 1 g:45 ml, stirred evenly, and then allowed to stand for 50 minutes.
[0087] (ii) After the above step (i) is completed, the solid product in the solution is filtered out, and then the solid product is washed twice with ethanol. After completion, the solid product is placed in an oven at 50° C. and dried until the moisture content is reduced to 5%, thereby obtaining the modified regenerated wood fiber.
[0088] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 4.46 MPa and 5.12 MPa, respectively.
[0089] Example 12
[0090] A preparation process of a recycled wood fiber cement-based repair material comprises the following steps:
[0091] (1) Prepare the following raw material components: 45 parts by weight of 42.5 silicate cement, 93 parts by weight of river sand, 11 parts by weight of pyrite magnetic separation tailings powder, 4 parts by weight of recycled wood fiber powder, 25 parts by weight of water, 0.9 parts by weight of water reducer, and 0.7 parts by weight of sucrose retarder. The pyrite magnetic separation tailings powder has a specific surface area of 800m 2 / kg of ultra-fine mineral powder. The particle size of the river sand is continuously graded between 0.5 and 1.5 mm. The water reducer is a naphthalene-based water reducer with a water reduction rate of 30%. The length of the regenerated wood fiber powder is approximately distributed between 200 and 350 μm.
[0092] (2) The cement, river sand, pyrite magnetic tailings powder, and recycled wood fiber powder are mixed and mechanically stirred for 10 minutes to obtain a dry mix, and then the water reducer, retarder, and water are added thereto and mechanically stirred for 5 minutes to obtain a repair material.
[0093] The tensile bonding strength and splitting strength of the test block repaired with the repair material prepared in this embodiment were tested using the same method as in the above-mentioned embodiment 1, and the results were 3.71 MPa and 4.26 MPa, respectively.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A recycled wood fiber cement-based repair material, characterized in that: The raw materials of the repair material include, by weight: 45-62 parts of cement, 93-117 parts of fine aggregate, 11-15 parts of pyrite magnetic separation tailings, 4-7.5 parts of recycled wood fiber, 25-37 parts of water, 0.9-1.4 parts of water reducer, and 0.7-1.1 parts of retarder; wherein: the pyrite magnetic separation tailings is an ultrafine mineral powder associated with pyrite, and its specific surface area is 500-800m 2 / kg; The regenerated wood fiber is a modified regenerated wood fiber, and its preparation process comprises the following steps: (1) Place the regenerated wood fiber in an aqueous solution containing triethanolamine, stir evenly and let stand; after completion, add Al 3+ Stir the source evenly and let it stand again; (2) After the above step (1) is completed, the solid product in the reaction system is separated, washed and dried to obtain the modified regenerated wood fiber.
2. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: The water reducer includes any one of a polycarboxylate water reducer, a naphthalene water reducer, an aliphatic water reducer and an aminosulfonate water reducer.
3. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: The retarder includes any one of lignin sulfonate, sucrose, glucose, gluconate and boric acid.
4. The regenerated wood fiber cement-based repair material according to claim 1, characterized in that: The fine aggregate includes any one of natural sand and artificial sand.
5. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: The particle size of the fine aggregate is continuously graded between 0.5 and 1.5 mm.
6. The regenerated wood fiber cement-based repair material according to claim 1, characterized in that: In step (1), the mass fraction of triethanolamine in the aqueous solution is 3-6%.
7. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: In step (1), the mass volume ratio of the regenerated wood fiber and the aqueous solution is 1 g: 30-50 ml.
8. The regenerated wood fiber cement-based repair material according to claim 1, characterized in that: In step (1), the length of the regenerated wood fiber is between 200 and 350 μm.
9. The regenerated wood fiber cement-based repair material according to claim 1, characterized in that: The regenerated wood fiber is wood fiber prepared from waste wood.
10. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: In step (1), the aqueous solution contains Al 3+ The mass fraction of the source is 10~15%.
11. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: The Al 3+ The source includes at least one of aluminum chloride, aluminum sulfate, aluminum nitrate, and aluminum acetate.
12. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: In step (1), the standing time is 40 to 60 minutes, and the second standing time is 30 to 45 minutes.
13. The recycled wood fiber cement-based repair material according to claim 1, characterized in that: In step (2), the solid product is washed with methanol or ethanol, and then dried at 40-60° C. until the moisture content of the solid product is no more than 5%, thereby obtaining the modified regenerated wood fiber.
14. The preparation process of the regenerated wood fiber cement-based repair material according to any one of claims 1 to 13, characterized in that: The steps include: (a) mixing the pyrite magnetic separation tailings and a portion of the water and stirring them for a period of time, and then mixing the resulting mixture with the cement, fine aggregate, recycled wood fiber or modified recycled wood fiber and stirring them for a period of time; (b) Then, add the water reducing agent, retarder and the remaining water and stir evenly to obtain the repair material.
15. The preparation process of the regenerated wood fiber cement-based repair material according to claim 14, characterized in that: In step (a), the pyrite magnetic separation tailings and 30-45% of the water are mixed and stirred for 10-20 minutes to obtain a mixed solution.
16. The process for preparing the regenerated wood fiber cement-based repair material according to claim 14, characterized in that: In step (a), the mixed liquid is mixed with cement, fine aggregate and recycled wood fiber and stirred continuously for 5 to 10 minutes.