Preparation method of sunlight-degradable TPE material and sunlight-degradable TPE material

By treating with silane coupling agents and glycerol oiling, combined with nano-titanium dioxide photodegradable agents, the problem of the difficulty in degrading TPE glove materials has been solved, achieving improved performance and environmental friendliness of TPE materials that can be degraded by sunlight.

CN116554632BActive Publication Date: 2026-11-10SHANGHAI NEW SHANGHUA POLYMER MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310719832.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-17
Publication Date
2026-11-10
Estimated Expiration
2043-06-17

AI Technical Summary

Technical Problem

Disposable TPE gloves are made of materials that are difficult to degrade in nature, leading to environmental pollution problems.

Method used

Thermoplastic starch and fillers are treated with silane coupling agents, combined with glycerol oil-extruded treatment and nano-titanium dioxide photodegradable agent, to improve the stability and degradation performance of the material by forming a non-polar molecular film and photodegradation mechanism.

Benefits of technology

Significant degradation of TPE materials under light irradiation was achieved, improving the tensile strength, tear strength and resilience of the materials. The degradation effect was remarkable, and the low temperature resistance and aging performance were excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004290924840000041
    Figure BDA0004290924840000041
  • Figure BDA0004290924840000051
    Figure BDA0004290924840000051
  • Figure BDA0004290924840000061
    Figure BDA0004290924840000061
Patent Text Reader

Abstract

This application relates to the field of biodegradable materials technology, and more specifically, to a method for preparing a sunlight-degradable TPE material and the sunlight-degradable TPE material itself. The method for preparing a sunlight-degradable TPE material includes the following steps: excipient pretreatment: treating thermoplastic starch and fillers with a silane coupling agent to obtain pretreated excipients; primary oiling: thoroughly grinding the matrix resin, adding heated first filler oil glycerol to the ground matrix resin, and mixing evenly to obtain a primary oiled raw material; secondary oiling: mixing the primary oiled raw material with lubricant, antioxidant, and photodegradant, adding a second filler oil, then adding the pretreated excipients and pigments, and mixing evenly to obtain a secondary oiled raw material; finished product: internally mixing and extruding the secondary oiled raw material to obtain the sunlight-degradable TPE material. Applying the TPE material obtained in this application to disposable gloves can solve the problem of the difficulty in degrading disposable glove materials in nature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of biodegradable materials technology, and more specifically, it relates to a method for preparing a sunlight-degradable TPE material and the sunlight-degradable TPE material. Background Technology

[0002] With the improvement of people's living standards, the use of disposable gloves has become increasingly widespread. Currently, disposable gloves on the market are made of materials such as latex gloves, nitrile gloves, PVC gloves, and TPE gloves. However, latex gloves offer poor protection against oils and synthetic organic compounds and pose a risk of protein allergies; nitrile gloves offer poor protection against ketones, aromatic compounds, and moderately polar compounds; and PVC gloves offer poor protection against organic solvents, which may allow some organic solvents to quickly penetrate the skin. TPE gloves offer good protection, are soft, abrasion-resistant, resistant to high and low temperatures, and safe, and have been popular since their invention. However, because these disposable materials are often disposed of carelessly after use and are difficult to degrade in nature, they cause many long-term, deep-seated, and serious ecological problems for human living environments. Summary of the Invention

[0003] To address the problem of the difficulty in degrading disposable TPE glove materials in nature, this application provides a method for preparing a sunlight-degradable TPE material and the sunlight-degradable TPE material itself.

[0004] In a first aspect, this application provides a method for preparing a sunlight-degradable TPE material, employing the following technical solution: A method for preparing a sunlight-degradable TPE material includes the following steps: Pretreatment of excipients: Thermoplastic starch and fillers are treated with silane coupling agents to obtain pretreated excipients; One-time oil filling: The matrix resin is thoroughly ground, and the heated first filler oil glycerol is added to the ground matrix resin and mixed evenly to obtain the one-time oil filling raw material; Secondary oil filling: After mixing the primary oil filling raw material with lubricant, antioxidant, and photodegradation agent, add the second filling oil, then add the pre-treated auxiliary materials and pigments, mix evenly, and obtain the secondary oil filling raw material; Finished product: The secondary oil-extruded raw material is intensively mixed, extruded and granulated to obtain a sun-degradable TPE material.

[0005] By adopting the above technical solution, pretreating thermoplastic starch and fillers with silane coupling agents can form a non-polar molecular film on the surface of the fillers and thermoplastic starch, making the fillers and thermoplastic starch hydrophobic, improving the stability, dispersibility and adhesion of thermoplastic starch and fillers in TPE materials, and enhancing the electrical, mechanical and weather resistance properties of TPE materials. At the same time, this non-polar molecular film on the surface of the fillers and thermoplastic starch reduces the friction between the fillers and thermoplastic starch, making the thermoplastic starch and fillers smooth and fluffy, and improving their processing performance. By using glycerol to perform a single oil-filling treatment on the matrix resin, glycerol can absorb moisture from the air. Under the combined action of trace amounts of moisture, silane coupling agents, and photodegrading agents, the photodegradability of TPE materials can be significantly improved. The matrix resin is ground and subjected to two oil filling processes, which reduces the particle size, increases the specific surface area, and ensures uniform mixing of the components in the raw materials. This results in TPE materials with greater tensile strength, tear strength, good resilience, low-temperature resistance, and aging resistance.

[0006] Preferably, the heating temperature of the glycerol is 50-100°C.

[0007] By adopting the above technical solution, when glycerol is heated to the above temperature, the components of the raw material can absorb glycerol more fully, resulting in a better oil filling effect and further improving the photodegradation performance of TPE materials.

[0008] Preferably, in the primary oil filling step, the diameter of the solid after grinding the matrix resin is less than 1 mm.

[0009] By adopting the above technical solution, when the solid diameter of the matrix resin after grinding is less than 1 mm, the particle size of the matrix resin is small and the specific surface area is large, which can fully absorb glycerol, so that the material has good photodegradation performance, large tensile strength, tear strength, good resilience, low temperature resistance and aging resistance.

[0010] Secondly, this application provides a sunlight-degradable TPE material, employing the following technical solution: A sun-degradable TPE material is prepared by the aforementioned method for preparing sun-degradable TPE materials; the sun-degradable TPE material comprises the following raw materials in parts by weight: The matrix resin comprises 5-250 parts, wherein the matrix resin comprises 10-100 parts of hydrogenated styrene-ethylene-butadiene-styrene block copolymer, 5-50 parts of polyethylene, 5-50 parts of polypropylene, and 5-50 parts of ethylene-octene copolymer. First filler oil: glycerol 2.5-50 parts; Second filler oil 2.5-50 parts; 5-50 parts of thermoplastic starch; 0.1-3.0 parts of silane coupling agent; Photodegradable agent 0.1-3.0 parts; Lubricant 0.01-3.0 parts; Antioxidant 0.1-3.0 parts; 1-50 parts of filler; Pigment 0.1-5.0 parts.

[0011] Preferably, the photodegrading agent is one or more of cerium stearate, ferric stearate, manganese stearate, ferric N-dibutyldithiocarbamate, nickel N,N-dibutyldithiocarbamate, and nano-titanium dioxide.

[0012] Preferably, the photodegrading agent is nano-titanium dioxide and / or cerium stearate.

[0013] By adopting the above technical solution, nano-titanium dioxide and cerium stearate have a synergistic effect in promoting the photodegradation of TPE materials.

[0014] Preferably, the sun-degradable TPE material further contains 0.05-0.1 parts of an accelerator, wherein the accelerator is one or more of ethylene glycol dimethyl ether, 1,4-dioxane, and n-butyl phthalate.

[0015] By adopting the above technical solution, nano-titanium dioxide, as a photodegrading agent, generates holes and electrons under light irradiation, producing active free radicals. These free radicals can break the molecular chains of TPE materials, thereby achieving the degradation of TPE materials. The above-mentioned promoters are good electron donors, which can inhibit the recombination of electrons and holes, achieve effective separation of holes and electrons, improve the photocatalytic activity of nano-titanium dioxide, and thus promote the degradation of TPE materials.

[0016] Preferably, the second filler oil is one or more of glycerol, naphthenic oil, hydrogenated naphthenic oil, and white oil.

[0017] Preferably, the thermoplastic starch is one or more of glycerol-plasticized thermoplastic starch, sorbitol-plasticized thermoplastic starch, and formamide-plasticized thermoplastic starch.

[0018] Preferably, the silane coupling agent is one or more of vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-aminopropyltriethoxysilane, and γ-(methacryloyloxy)propyltrimethoxysilane.

[0019] In summary, this application has the following beneficial effects: 1. This application uses a silane coupling agent to pretreat thermoplastic starch and fillers. On the one hand, this can improve the stability and dispersibility of thermoplastic starch and fillers in TPE materials, thereby improving the mechanical and weather resistance properties of TPE materials. On the other hand, the non-polar molecular film on the surface of the filler and thermoplastic starch reduces the friction between the filler and thermoplastic starch, making the thermoplastic starch and filler smooth and fluffy, thus improving their processing performance.

[0020] 2. This application utilizes glycerol to perform a single oil-filling treatment on the matrix resin. Glycerol can absorb moisture from the air, and under the combined action of trace amounts of moisture, silane coupling agents, and photodegrading agents, it can significantly improve the photodegradation performance of TPE materials.

[0021] 3. This application grinds and oil-fills the matrix resin twice, which reduces the particle size, increases the specific surface area, and makes the components in the raw material more uniformly mixed, so that the TPE material has greater tensile strength, tear strength, better resilience, low temperature resistance, and aging resistance.

[0022] 4. This application uses nano-titanium dioxide as a photodegrading agent and adds ethylene glycol dimethyl ether, 1,4-dioxane, and n-butyl phthalate as promoters. Nano-titanium dioxide has good photodegradation performance. Under light irradiation, it generates holes and electrons, producing active free radicals. These free radicals can break the molecular chains of TPE materials, thereby achieving the degradation of TPE materials. The above promoters are good electron donors, which can inhibit the recombination of electrons and holes, achieve effective separation of holes and electrons, improve the photocatalytic activity of nano-titanium dioxide, and thus effectively promote the degradation of TPE materials. Detailed Implementation

[0023] The present application will be further described in detail below with reference to the embodiments.

[0024] Unless otherwise specified, the specifications of the raw materials used in the following examples and comparative examples are detailed in Table 1.

[0025] Table 1. Raw material specifications information Preparation example of modified nano titanium dioxide Preparation Example 1 Modified nano-titanium dioxide was prepared according to the following steps: 500g of nano-titanium dioxide was added to 2kg of anhydrous ethanol and ultrasonically dispersed for 30min to obtain dispersed nano-titanium dioxide; 1kg of γ-methacryloxypropyltrimethoxysilane was dissolved in 2kg of deionized water and hydrolyzed for 30min to obtain hydrolyzed silane coupling agent; the dispersed nano-titanium dioxide and the hydrolyzed silane coupling agent were mixed and stirred at 70℃ for 2h, filtered and dried to obtain modified nano-titanium dioxide. Example

[0026] Example 1 A photodegradable TPE material, the formulation of which is as follows: 10 kg of hydrogenated styrene-ethylene-butadiene-styrene block copolymer 5kg of polyethylene 5kg of polypropylene 5kg of ethylene octene copolymer First filler oil: glycerol 2.5 kg Second filler oil: naphthenic oil 2.5kg 5 kg of sorbitol-plasticized thermoplastic starch. Silane coupling agent vinyltriethoxysilane 0.1kg Photodegradable agent ferric stearate 0.1kg, Lubricant oleamide 0.01kg, Antioxidant pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid) ester 0.1 kg 1 kg of filler talc powder 0.1 kg of ultramarine pigment.

[0027] A photodegradable TPE material is prepared according to the following steps: Weigh each component precisely and set aside for later use; Excipient pretreatment: Dissolve the silane coupling agent in anhydrous ethanol to prepare a 5 wt% treatment solution. Add the thermoplastic starch and filler together to a high-speed mixing pot, and slowly add the treatment solution while stirring slowly using a spray device. After 10 minutes, when the thermoplastic starch and filler become smooth and fluffy, release the mixture to obtain the pretreated excipient. First-stage oil filling: The first filling oil, glycerol, is heated to 50°C. Hydrogenated styrene-ethylene-butadiene-styrene block copolymer (SEBS), polyethylene (PE), polypropylene (PP), and ethylene octene copolymer (POE) are added together in a colloid mill and ground thoroughly until the solid diameter is less than 1 mm. The heated glycerol is then slowly added. After 10 minutes, a uniformly mixed material is obtained. After standing for 24 hours, the first-stage oil filling raw material is obtained. Secondary oil filling: Add the settled primary oil filling raw material, lubricant, antioxidant, photodegradation agent, etc. into the medium-high speed mixing pot, start the high speed mixing pot, and slowly add the second filling oil naphthenic oil after 1 minute. After 10 minutes, add the pre-treated auxiliary materials and pigments into the high speed mixing pot. After 10 minutes, a uniformly mixed secondary oil filling raw material is obtained. Internal mixing: The secondary oil-filled raw material is mixed using an internal mixer to obtain a well-mixed agglomerated material. The temperature parameters of the internal mixing chamber are set to 180℃ and the rotor speed of the internal mixing chamber is 60 rpm. Extruder granulation: The lumps that have been mixed by the internal mixer are extruded and granulated through an extruder. The parameters of the extruder are set as follows: zone 1 temperature 150℃, zone 2 temperature 160℃, zone 3 temperature 170℃, die head temperature 185℃, and main engine frequency 50HZ. Uniform, sun-degradable TPE material is obtained from the extruder.

[0028] Example 2 A solar-degradable TPE material differs from Example 1 in that the heating temperature of glycerol is different; in this example, the heating temperature of glycerol is 100°C.

[0029] Example 3 A solar-degradable TPE material differs from Example 1 in that the heating temperature of glycerol is different; in this example, the heating temperature of glycerol is 75°C.

[0030] Examples 4-5 A sun-degradable TPE material differs from Example 1 in that its raw material composition is different, as shown in Table 2 below: Table 2. Raw material composition of solar biodegradable TPE materials Example 6 A photodegradable TPE material differs from Example 1 in that the photodegrading agent is different; in this example, iron stearate is replaced with cerium stearate.

[0031] Example 7 A photodegradable TPE material is different from Example 1 in that the photodegrading agent is different. In this example, iron stearate and other materials are replaced with the modified nano titanium dioxide prepared in Example 1.

[0032] Example 8 A photodegradable TPE material differs from Example 7 in that: 0.05 kg of ethylene glycol dimethyl ether is added to the raw materials of the photodegradable TPE material, and the ethylene glycol dimethyl ether is added at the same time as the photodegrading agent.

[0033] Example 9 A photodegradable TPE material differs from Example 7 in that: 0.1 kg of 1,4-dioxane is added to the raw materials of the photodegradable TPE material, and 1,4-dioxane is added simultaneously with the photodegrading agent.

[0034] Example 10 A photodegradable TPE material differs from Example 7 in that: 0.08 kg of n-butyl phthalate is added to the raw materials of the photodegradable TPE material, and n-butyl phthalate is added at the same time as the photodegrading agent.

[0035] Example 11 A solar-degradable TPE material differs from Example 1 in that the second filling oil in the secondary oiling step is different; in this example, cycloalkane oil is replaced by glycerol.

[0036] Example 12 A photodegradable TPE material differs from Example 1 in that the choice of thermoplastic starch is different. In this example, the sorbitol-plasticized thermoplastic starch is replaced with glycerol-plasticized thermoplastic starch.

[0037] Example 13 A photodegradable TPE material differs from Example 1 in that the silane coupling agent is different; in this example, vinyltriethoxysilane is replaced by vinyltrimethoxysilane.

[0038] Example 14 A sun-degradable TPE material differs from Example 1 in that the heating temperature of glycerol is different; in this example, the heating temperature of glycerol is 30°C.

[0039] Example 15 A solar-degradable TPE material differs from Example 1 in that the heating temperature of glycerol is different; in this example, the heating temperature of glycerol is 150°C.

[0040] Example 16 A photodegradable TPE material differs from Example 1 in that the photodegrading agent is different. In this example, the photodegrading agent is 0.05 kg of cerium stearate and 0.05 kg of modified nano-titanium dioxide prepared in Example 1.

[0041] Example 17 The difference between this solar biodegradable TPE material and Example 1 is that the solid diameters of the hydrogenated styrene-ethylene-butadiene-styrene block copolymer (SEBS), polyethylene (PE), polypropylene (PP), and ethylene octene copolymer (POE) after grinding are different in the single oil filling step. The solid diameter in this example is 1-10 mm.

[0042] Comparative Example Comparative Example 1 A sunlight-degradable TPE material differs from Example 1 in that its preparation method is different, and the specific steps are as follows: Weigh each component precisely and set aside for later use; First-stage oil filling: The first filling oil, glycerol, is heated to 50°C. Hydrogenated styrene-ethylene-butadiene-styrene block copolymer (SEBS), polyethylene (PE), polypropylene (PP), and ethylene octene copolymer (POE) are added together in a colloid mill and ground thoroughly until the solid diameter is less than 1 mm. The heated glycerol is then slowly added. After 10 minutes, a uniformly mixed material is obtained. After standing for 24 hours, the first-stage oil filling raw material is obtained. Secondary oil filling: Add the settled primary oil filling raw material, lubricant, antioxidant, photodegradation agent, etc. into the medium-high speed mixing pot. Start the high speed mixing pot. After 1 minute, slowly add the second filling oil naphthenic oil. After 10 minutes, add thermoplastic starch, filler and pigment into the high speed mixing pot. After 10 minutes, a uniformly mixed secondary oil filling raw material is obtained. Internal mixing: The secondary oil-filled raw material is mixed using an internal mixer. The internal mixing chamber temperature is set to 180℃ and the internal mixing chamber rotor speed is 60 rpm. When the internal mixing chamber temperature reaches the set temperature, the well-mixed lumps are obtained. Extruder granulation: The lumps that have been mixed by the internal mixer are extruded and granulated through an extruder. The parameters of the extruder are set as follows: zone 1 temperature 150℃, zone 2 temperature 160℃, zone 3 temperature 170℃, die head temperature 185℃, and main machine frequency 50Hz. Uniform, sun-degradable TPE material is obtained from the extruder.

[0043] Comparative Example 2 A sun-degradable TPE material differs from Example 1 in that the first filler oil is different; in this comparative example, glycerol is replaced by naphthenic oil.

[0044] Comparative Example 3 A sun-degradable TPE material differs from Example 11 in that the first filler oil is different; in this comparative example, glycerol is replaced by naphthenic oil.

[0045] Detection methods Referring to GB / T 20197, the photodegradable TPE materials prepared in Examples 1-17 and Comparative Examples 1-3 were exposed to xenon lamp accelerated aging chamber for 90 days, and their relevant properties were tested. The specific test results are shown in Table 3 below: Table 3. Performance Tests of Sun-Degradable TPE Materials As shown in Table 3, the photodegradable TPE material prepared in this application, after being exposed to xenon lamp artificial aging chamber for 90 days, exhibits a tensile elongation at break retention rate (longitudinal / transverse) (%) ≤ 5, a weight-average relative molecular mass decrease rate (%) ≥ 78, and a molecular percentage content (%) of weight-average relative molecular mass < 10000 after photodegradation ≥ 22, all meeting the requirements of GB / T 20197. This indicates that the photodegradable TPE material prepared in this application exhibits significant degradation effect after being exposed to xenon lamp artificial aging chamber for 90 days.

[0046] Combining Example 1 and Comparative Example 1 with Table 3, it can be seen that after 90 days of exposure in a xenon lamp artificial aging chamber, the retention rate of tensile elongation at break (longitudinal / transverse) of the photodegradable TPE material prepared in Example 1 is much smaller than that in Comparative Example 1. Furthermore, the decrease rate of weight-average relative molecular mass (%) and the percentage of molecules with weight-average relative molecular mass <10000 after photodegradation (%) are both much larger than those in Comparative Example 1. This indicates that the degradation effect of Example 1 is far superior to that of Comparative Example 1. This may be because: the preparation steps of Example 1 include excipient pretreatment, that is, pretreating thermoplastic starch and filler with silane coupling agent. The silane coupling agent can work together with glycerol, trace moisture and photodegrading agent to significantly improve the photodegradation performance of TPE material; in addition, it can also form a non-polar molecular film on the surface of filler and thermoplastic starch, making filler and thermoplastic starch hydrophobic, improving the stability, dispersibility and adhesion of thermoplastic starch and filler in TPE material, and improving the electrical, mechanical and weather resistance properties of TPE material; at the same time, this non-polar molecular film on the surface of filler and thermoplastic starch reduces the friction between filler and thermoplastic starch, making thermoplastic starch and filler smooth and fluffy, improving its processing performance.

[0047] Combining Example 1 and Comparative Example 2 with Table 3, it can be seen that the photodegradable TPE material prepared in Example 1, after being exposed to xenon lamp artificial aging chamber for 90 days, exhibited a significantly lower retention rate of tensile elongation at break (longitudinal / transverse) (%) than that in Comparative Example 2. Furthermore, the decrease in weight-average relative molecular mass (%) and the percentage of molecules with a weight-average relative molecular mass <10000 after photodegradation (%) were both significantly higher in Example 1 than in Comparative Example 2. This indicates that the degradation effect of Example 1 is far superior to that of Comparative Example 2. This may be because Comparative Example 2 did not use glycerol as the first filler oil, while Example 1 did. The authors unexpectedly discovered that glycerol can absorb moisture from the air, and under the combined action of trace amounts of moisture, silane coupling agents, and photodegrading agents, it can significantly improve the photodegradation performance of the TPE material.

[0048] Combining Examples 1, 11, and Comparative Example 3 with Table 3, it can be seen that the retention rate of tensile elongation at break (longitudinal / transverse) (%) of the photodegradable TPE materials prepared in Examples 1 and 11 after 90 days of exposure in a xenon lamp artificial aging chamber is much lower than that in Comparative Example 3. Furthermore, the decrease rate (%) of weight-average relative molecular mass and the percentage of molecules with a weight-average relative molecular mass <10000 after photodegradation are both much higher than in Comparative Example 3. This indicates that the degradation effect of Examples 1 and 11 is far superior to that of Comparative Example 3. This may be because: Comparative Example 3 did not use glycerol as the first filler oil, while Examples 1 and 11 did use glycerol. Glycerol can absorb moisture from the air, and under the combined action of trace moisture, silane coupling agent, and photodegrading agent, it can significantly improve the photodegradation performance of the TPE material. Even though Comparative Example 3 used glycerol as the second filler oil, it could not achieve the degradation effect of Examples 1 and 11.

[0049] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A photodegradable TPE material, characterized in that: The solar-degradable TPE material comprises the following raw materials in parts by weight: The matrix resin comprises 25-250 parts, wherein the matrix resin comprises 10-100 parts of hydrogenated styrene-ethylene-butadiene-styrene block copolymer, 5-50 parts of polyethylene, 5-50 parts of polypropylene, and 5-50 parts of ethylene-octene copolymer. First filler oil: glycerol 2.5-50 parts; Second filler oil 2.5-50 parts; 5-50 parts of thermoplastic starch; 0.1-3.0 parts of silane coupling agent; Photodegradable agent 0.1-3.0 parts; Lubricant 0.01-3.0 parts; Antioxidant 0.1-3.0 parts; 1-50 parts of filler; Pigment 0.1-5.0 parts; The photodegrading agent is one or more of cerium stearate, ferric stearate, manganese stearate, and nano titanium dioxide; The second filler oil is one or more of glycerol, naphthenic oil, hydrogenated naphthenic oil, and white oil; The thermoplastic starch is one or more of glycerol-plasticized thermoplastic starch, sorbitol-plasticized thermoplastic starch, and formamide-plasticized thermoplastic starch. The silane coupling agent is one or more of vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-aminopropyltriethoxysilane, and γ-(methacryloyloxy)propyltrimethoxysilane.

2. The photodegradable TPE material according to claim 1, characterized in that: The solar-degradable TPE material also contains 0.05-0.1 parts of an accelerator, wherein the accelerator is one or more of ethylene glycol dimethyl ether and 1,4-dioxane.

3. A method for preparing the solar-degradable TPE material according to claim 1, characterized in that: Includes the following steps: Pretreatment of excipients: Thermoplastic starch and fillers are treated with silane coupling agents to obtain pretreated excipients; One-time oil filling: The matrix resin is thoroughly ground, and the heated first filler oil glycerol is added to the ground matrix resin and mixed evenly to obtain the one-time oil filling raw material; Secondary oil filling: After mixing the primary oil filling raw material with lubricant, antioxidant, and photodegradation agent, add the second filling oil, then add the pre-treated auxiliary materials and pigments, mix evenly, and obtain the secondary oil filling raw material; Finished product: The secondary oil-extruded raw material is intensively mixed, extruded and granulated to obtain a sun-degradable TPE material.

4. The method for preparing the sunlight-degradable TPE material according to claim 3, characterized in that: The heating temperature of the glycerol is 50-100℃.

5. The method for preparing the sunlight-degradable TPE material according to claim 3, characterized in that: In the first oil filling step, the diameter of the solid after grinding the matrix resin is less than 1 mm.

Citation Information

Patent Citations

  • Degradable environmental-friendly rubber glove and preparation method thereof

    CN108250471A

  • Biodegradable thermoplastic elastomer material and preparation method thereof

    CN110229471A