A magnetic tunnel junction array and its fabrication method

By employing a synergistic etching technique combining cyano radicals and inert gas ions, the problem of shadowing effect in the etching of high-density magnetic tunnel junction arrays was solved, achieving efficient and uniform material removal, which is suitable for fabricating high-density MRAM memories.

CN116568120BActive Publication Date: 2026-11-17BEIJING SUPERSTRING ACAD OF MEMORY TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210106393.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2026-11-17
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

Existing reactive ion etching and ion beam etching techniques are difficult to effectively etch magnetic tunnel junction arrays, especially at high densities where shadowing effects are prone to occur, leading to uneven etching and low material removal efficiency.

Method used

The synergistic etching technique using cyano radicals and inert gas ions is employed to achieve efficient material removal by chemically reacting and modifying cyano radicals formed in plasma with magnetic tunnel junction and hard mask layer materials, followed by physical bombardment using inert gas ions.

Benefits of technology

It effectively reduces or avoids the shadowing effect, improves the uniformity and efficiency of etching, and is suitable for fabricating high-density magnetic tunnel junction arrays, especially MTJ arrays with diameters of Sub-80nm, Sub-70nm, Sub-60nm or Sub-50nm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116568120B_ABST
    Figure CN116568120B_ABST
Patent Text Reader

Abstract

A magnetic tunnel junction array and its fabrication method are disclosed. The fabrication method includes: S10: providing a substrate; S20: forming a bottom electrode layer, a magnetic tunnel junction layer, and a hard mask layer on the substrate; S30: patterning the magnetic tunnel junction layer and the hard mask layer; S40: forming cyano radicals in plasma using a cyano radical precursor gas, chemically reacting the cyano radicals with the materials of the magnetic tunnel junction layer and the hard mask layer, and / or chemically modifying the materials of the magnetic tunnel junction layer and the hard mask layer using cyano radicals, and removing the chemical reaction products and / or the chemically modified materials and / or the unreacted and unmodified materials of the magnetic tunnel junction layer and the hard mask layer using inert gas ions, thereby obtaining a magnetic tunnel junction array. The fabrication method of this application can reduce or avoid the shadowing effect problem, which is beneficial for the miniaturization of MTJs and the fabrication of high-density MRAM memories.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor devices, and more particularly to a magnetic tunnel junction array and its fabrication method. Background Technology

[0002] Magnetic Random Access Memory (MRAM) is a random access memory that stores data using magnetoresistive properties. It features high-speed read / write, large capacity, and low power consumption. The core storage device of MRAM is the magnetic tunnel junction (MTJ).

[0003] Currently, the mainstream semiconductor etching process is reactive ion etching (RIE). When etching polysilicon or metals, halogen gases (such as Cl2) are typically used as the main etching gas. The halogen gas forms halogen radicals in the plasma, which then react chemically with the material to be etched. The reaction products are then removed, thus achieving etching. However, some materials that form MTJs (Metal-to-Jet Layers), such as Fe, Co, Mg, Ru, Pt, Pd, Al, Rh, Mo, Ni, or Ir, do not react with the halogen radicals formed in the plasma, or are very difficult to remove. Furthermore, the subsequent dehalogenation process introduces H2O, which is unacceptable in MTJ manufacturing. Therefore, traditional RIE is not suitable for etching MTJ arrays.

[0004] Currently, low-density MTJ arrays generally employ ion beam etching (IBE). IBE utilizes the glow discharge principle to ionize argon gas into Ar. + Ar + The sample surface is physically bombarded by the acceleration of the anodic electric field to achieve the etching effect. Figure 1 This shows the sputtering rate and deposition rate as a function of the incident angle during the etching process of a specific etching front-end 10 using IBE. Figure 1 As shown, since the byproducts of IBE are not gases, they will be redeposited, making IBE a dynamic equilibrium process of sputtering and deposition. For a specific etch front 10, the sputtering rate will increase with the amount of Ar. + The deposition rate does not change with the incident angle θ of Ar, but rather with the change in Ar incidence angle θ. + The deposition rate varies with the incident angle of Ar. However, it is not constant; it is strongly correlated with the surrounding environment of the specific etch front 10 and changes dynamically over time. To obtain a higher sputtering rate, Ar is generally used... +The incident direction of Ar will maintain an angle θ with the normal of the etching front-end 10, especially when the deposition rate is high. For a specific etching front-end 10, when the deposition rate is greater than the sputtering rate, the Ar angle can be increased. + Or, by adjusting the angle θ of the Ar incident direction, the sputtering rate is increased, thereby achieving material removal at a specific etching front 10. However, as Figure 2 As shown, as the geometry of the etched region decreases, Ar + The space for increasing the angle θ of the Ar incident direction is limited, meaning that the increased sputtering rate resulting from increasing the angle θ cannot exceed the deposition rate, thus failing to meet the material removal conditions of the specific etching front-end 10. In this case, "material removal" (i.e., etching) will stop, and the specific etching front-end 10 will be at the Ar angle θ where material can be removed. + Or in the shadow of an Ar beam, this effect is called the shadowing effect. Figure 2 This is a schematic diagram illustrating the formation principle of the shadowing effect. Due to the presence of the shadowing effect, IBE is not the optimal etching solution for high-density MTJ arrays. Summary of the Invention

[0005] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.

[0006] This application provides a method for fabricating a magnetic tunnel junction array. This method can reduce or avoid the shadowing effect problem faced by IBE etching of high-density MTJ arrays, which is beneficial for the miniaturization of MTJs and the fabrication of high-density MRAM memories.

[0007] This application provides a method for fabricating a magnetic tunnel junction array, the method comprising:

[0008] S10: Provides a substrate;

[0009] S20: A bottom electrode layer, a magnetic tunnel junction layer, and a hard mask layer are sequentially formed on the substrate;

[0010] S30: Pattern the magnetic tunneling layer and the hard mask layer;

[0011] S40: The precursor gas of cyano radicals is used to form cyano radicals in plasma. The cyano radicals are then chemically reacted with the materials of the patterned magnetic tunnel junction layer and hard mask layer, and / or the materials of the patterned magnetic tunnel junction layer and hard mask layer are chemically modified using cyano radicals. The ion source gas of the inert gas ions is then used to form inert gas ions. The chemical reaction products and / or the chemically modified materials and / or the unreacted and unmodified materials of the patterned magnetic tunnel junction layer and hard mask layer are then removed using the inert gas ions to obtain a magnetic tunnel junction array.

[0012] In embodiments of this application, the material of the magnetic tunnel layer may include any one or more of iron, cobalt, cobalt-iron-boron, nickel, tungsten, molybdenum, chromium, ruthenium, iridium, palladium, platinum, magnesium oxide, aluminum, zinc, titanium, and rhodium.

[0013] In embodiments of this application, the material of the hard mask layer may be selected from tantalum and tantalum nitride, or any one or more of them.

[0014] In the embodiments of this application, the precursor gas of the cyano radical can be selected from any one or more of HCN, (CN)2, CH3CN, CH4 / NH3, CH3OH / NH3 and CH3CH2OH / NH3.

[0015] In the embodiments of this application, the pressure during the chemical reaction and / or the chemical modification can be 0.3 mTorr-10 mTorr.

[0016] In the embodiments of this application, the ion source gas of the inert gas ions may include any one or more of neon, argon, krypton, and xenon, and may add any one or more of CO, CO2, N2, O2, and He as a carrier gas.

[0017] In the embodiments of this application, the total flow rate of the precursor gas of the cyano radical and the ion source gas of the inert gas ions can be 100 sccm-2000 sccm.

[0018] In embodiments of this application, the power of the radio frequency source power supply that generates and sustains the plasma can be 100 watt to 3000 watt.

[0019] In an embodiment of this application, the frequency of the radio frequency power source can be 13.56MHz.

[0020] In embodiments of this application, the removal of chemical reaction products and / or chemically modified materials and / or unreacted and unmodified patterned magnetic tunnel junction layers and hard mask layers using the inert gas ions may include: accelerating the inert gas ions using a radio frequency bias power supply, and bombarding the chemical reaction products and / or chemically modified materials and / or unreacted and unmodified patterned magnetic tunnel junction layers and hard mask layers with the accelerated inert gas ions to remove the materials.

[0021] In the embodiments of this application, the ion acceleration voltage provided by the radio frequency bias power supply can be 30V-1000V.

[0022] In the embodiments of this application, the frequency of the radio frequency bias power supply can be 13.56MHz, 2MHz or 400kHz, preferably 400kHz.

[0023] In embodiments of this application, step S40 can be performed in an inductively coupled plasma etching cavity.

[0024] In the embodiments of this application, the preparation method may further include: trimming the sidewalls of the magnetic tunnel junction by ion beam etching during and / or after step S40 is completed to obtain the magnetic tunnel junction array.

[0025] In the embodiments of this application, the ion source gas for ion beam etching can be selected from any one or more of neon, argon, krypton, and xenon.

[0026] This application also provides a magnetic tunnel junction array, which is obtained by the preparation method described above.

[0027] In the embodiments of this application, the diameter of the magnetic tunnel junction of the magnetic tunnel junction array can be sub-80nm, sub-70nm, sub-60nm, or sub-50nm.

[0028] The method for fabricating the magnetic tunnel junction array in this application employs cyano radicals and inert gas ions for synergistic etching. Since the chemical reaction and modification are isotropic, the sticking coefficient of the chemical etching byproducts is smaller than that of physical etching. This effectively reduces or even avoids the shadowing effect problem of IBE etching. Simultaneously, the inert gas ions physically bombard materials that have undergone chemical reaction and / or modification, as well as those that have not, significantly increasing removal efficiency. Therefore, the method for fabricating the magnetic tunnel junction array in this application facilitates the miniaturization of MTJs and is suitable for fabricating high-density MRAM memories, such as MTJ arrays with diameters of Sub-80nm, Sub-70nm, Sub-60nm, or Sub-50nm.

[0029] Other features and advantages of this application will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the application. Other advantages of this application can be realized and obtained by means of the solutions described in the description and the accompanying drawings. Attached Figure Description

[0030] The accompanying drawings are used to provide an understanding of the technical solutions of this application and constitute a part of the specification. They are used together with the embodiments of this application to explain the technical solutions of this application and do not constitute a limitation on the technical solutions of this application.

[0031] Figure 1 The sputtering rate and deposition rate as a function of incident angle during the etching process of a specific etching front end using IBE;

[0032] Figure 2 This is a schematic diagram illustrating the formation principle of the shadow effect;

[0033] Figure 3 A diagram showing metals capable of chemically reacting with and / or being chemically modified by cyano radicals, and the reaction products;

[0034] Figure 4 This is a schematic diagram illustrating the process of step S40.

[0035] Figure 5 This is a schematic diagram of the ICP etching cavity and a graph showing the variation of ion energy distribution with ion flux under different RF bias power supply frequencies.

[0036] Figure 6 This is a schematic flowchart of the method for preparing the magnetic tunnel junction array of Embodiment 1 of this application.

[0037] The symbols in the attached diagram have the following meanings:

[0038] 10 - Etching front end; 20 - Gas inlet; 30 - RF source power supply; 40 - RF bias power supply; 50 - Throttle position sensor with throttle valve; 60 - Plasma; 70 - Wafer; 100 - Substrate; 110 - Dielectric; 120 - Via; 210 - Bottom electrode layer; 210' - Bottom electrode; 220 - Magnetic tunnel junction layer; 220' - Magnetic tunnel junction; 230 - Hard mask layer; 230' - Top electrode; 240 - Insulating layer. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application will be described in detail below with reference to the accompanying drawings. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be arbitrarily combined with each other.

[0040] This application provides a method for fabricating a magnetic tunnel junction array, including:

[0041] S10: Provides a substrate;

[0042] S20: A bottom electrode layer, a magnetic tunnel junction layer, and a hard mask layer are sequentially formed on the substrate;

[0043] S30: Pattern the magnetic tunneling layer and the hard mask layer;

[0044] S40: The precursor gas of cyano radicals is used to form cyano radicals in plasma. The cyano radicals are then chemically reacted with the materials of the patterned magnetic tunnel junction layer and hard mask layer, and / or the materials of the patterned magnetic tunnel junction layer and hard mask layer are chemically modified using cyano radicals. The ion source gas of the inert gas ions is then used to form inert gas ions. The chemical reaction products and / or the chemically modified materials and / or the unreacted and unmodified materials of the patterned magnetic tunnel junction layer and hard mask layer are then removed using the inert gas ions to obtain a magnetic tunnel junction array.

[0045] The method for fabricating magnetic tunnel junction arrays in this application employs synergistic etching using cyano radicals and inert gas ions (including chemically reacting and / or modifying the materials of the patterned magnetic tunnel junction layer and hard mask layer with cyano radicals, and physically bombarding the materials with inert gas ions to achieve synergistic etching). Since the chemical reaction and modification are isotropic, the sticking coefficient of the chemical etching byproducts is smaller than that of the physical etching, which effectively reduces or even avoids the shadowing effect problem of IBE etching. Simultaneously, the removal efficiency is greatly increased by physically bombarding the materials that have undergone chemical reaction and / or modification, as well as those that have not, with inert gas ions. Therefore, the method for fabricating magnetic tunnel junction arrays in this application facilitates the miniaturization of MTJs and is suitable for fabricating high-density MRAM memories, such as MTJ arrays with diameters of Sub-80nm, Sub-70nm, Sub-60nm, or Sub-50nm.

[0046] In embodiments of this application, the substrate may be a CMOS substrate.

[0047] In embodiments of this application, the material of the magnetic tunnel layer may include any one or more of the following: iron (Fe), cobalt (Co), cobalt-iron-boron (CoFeB), nickel (Ni), tungsten (W), molybdenum (Mo), chromium (Cr), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), magnesium oxide (MgO), aluminum (Al), zinc (Zn), titanium (Ti), and rhodium (Rh).

[0048] Currently, the materials constituting magnetic tunnel junctions (MTJs) are heavy metals or magnetic metals, such as iron (Fe), cobalt (Co), nickel (Ni), tungsten (W), molybdenum (Mo), chromium (Cr), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), magnesium (Mg), aluminum (Al), zinc (Zn), titanium (Ti), rhodium (Rh), and tantalum (Ta). The inventors of this application discovered during their research on magnetic tunnel junctions that conventional free radicals formed in plasma are very difficult to chemically react with or modify these materials. However, cyano radicals (-C≡N, Cyano-Group Radical) formed in plasma can chemically react with and / or modify other metals except Ta.

[0049] Figure 3 This document presents a diagram summarizing the metals and reaction products capable of chemically reacting with and / or modifying cyano radicals, as compiled by the inventors of this application. Figure 3As shown, cyano radicals formed in plasma can undergo complexation chemical reactions and / or chemical modifications with inert metals such as Fe, Co, Ni, Mg, Pt, Pd, Al, Zn, Ru, Ir, W, Ti, Rh, and Mo to generate Fe(CN)3, Co(CN)2, Co(CN)3, Ni(CN)2, Mg(CN)2, Pd(CN)2, Al(CN)3, Zn(CN)2, Pt(CN)2, Ru(CN)3, Ir(CN)3, W(CN)4, Ti(CN)4, Rh(CN)3, and Mo(CN)4. Figure 4 This is a schematic diagram of the process of step S40.

[0050] In the current mainstream MTJ main stack layer, Ta has been abandoned as an interlayer coupling layer material (Ta as an interlayer coupling layer cannot withstand 400℃ CMOS back-end annealing process); and since Ta does not chemically react or chemically modify with cyano radicals, it can be used as an MTJ hard mask (HM) layer material.

[0051] In embodiments of this application, the material of the hard mask layer may be selected from any one or more of tantalum (Ta) and tantalum nitride (TaN).

[0052] In embodiments of this application, the precursor gas for cyano radicals can be selected from any one or more of HCN, (CN)2, CH3CN, CH4 / NH3, CH3OH / NH3, and CH3CH2OH / NH3. These gases can generate cyano radicals in plasma, for example, a plasma formed by the precursor gas for cyano radicals and an inert gas.

[0053] In the embodiments of this application, the pressure during the chemical reaction and / or the chemical modification can be 0.3 mTorr-10 mTorr.

[0054] In the embodiments of this application, the ion source gas for the inert gas ions may include any one or more of neon, argon, krypton, and xenon, and may add any one or more of CO, CO2, N2, O2, and He as a carrier gas.

[0055] In step S40, to achieve a better removal effect, a turbocharged molecular pump (TMP) with high suction power and a large gas flow rate (including the precursor gas of the cyano radical and the ion source gas of the inert gas ions) can be selected. In the embodiments of this application, the total flow rate of the precursor gas of the cyano radical and the ion source gas of the inert gas ions can be 100 sccm-2000 sccm.

[0056] In embodiments of this application, the power of the radio frequency (RF) source power supply that generates and sustains the plasma can be between 100 watts and 3000 watts. In embodiments of this application, the frequency of the RF source power supply can be 13.56 MHz.

[0057] In embodiments of this application, the removal of chemical reaction products and / or chemically modified materials and / or unreacted and unmodified patterned magnetic tunnel junction layers and hard mask layers using the inert gas ions may include: accelerating the inert gas ions using an RF bias power supply, and bombarding the chemical reaction products and / or chemically modified materials and / or unreacted and unmodified patterned magnetic tunnel junction layers and hard mask layers with the accelerated inert gas ions to remove the materials.

[0058] In the embodiments of this application, the ion acceleration voltage provided by the radio frequency bias power supply can be 30V-1000V.

[0059] In the embodiments of this application, the ion acceleration voltage can be a pulsed bias voltage, that is, repeatedly cycling between applying a bias voltage and not applying a bias voltage. Based on a series of concepts similar to atomic layer etching (ALE), such as repeated cycles of chemical reaction and / or chemical modification and simple physical etching, better etching effect can be obtained.

[0060] In the embodiments of this application, the frequency of the radio frequency bias power supply can be 13.56MHz, 2MHz or 400kHz, preferably 400kHz.

[0061] In the embodiments of this application, in order to reduce the redeposition of reaction byproducts, their residence time (G) must be reduced. res ), where: Г res =PV / flow=V / C sccm / mTorr P is the working pressure, V is the volume of the reaction chamber, flow is the gas flow rate, and C is the pressure. sccm / mTorr It is a key indicator of the suction force of the etching cavity.

[0062] In embodiments of this application, step S40 can be performed in an inductively coupled plasma (ICP) etching cavity. Figure 5 This diagram shows the structure of an ICP etching chamber and the variation of ion energy distribution with ion flux at different RF bias power supply frequencies. Figure 5As shown in the left figure, the ICP etching chamber includes a gas inlet 20, an RF power supply 30, an RF bias power supply 40, and a throttle position sensor 50 with a throttle valve. The precursor gas of cyano radicals and the ion source gas (including the carrier gas) of inert gas ions enter the interior of the ICP etching chamber through the gas inlet 20. The inert gas is ionized to form plasma 60 (including inert gas ions). The precursor gas of cyano radicals forms cyano radicals in the plasma. In the ICP etching chamber, cyano radicals and inert gas ions are used to perform synergistic etching on the wafer 70 (wafer, which can be 300 mm in diameter).

[0063] In embodiments of this application, the material of the bottom electrode may be selected from any one or more combinations of titanium (Ti) and titanium nitride (TiN).

[0064] In an embodiment of this application, step S20 may include: after forming the bottom electrode layer and before forming the magnetic tunnel junction layer, performing a chemical mechanical planarization (CMP) process to planarize the bottom electrode layer in order to obtain the planarization requirements for fabricating the MTJ cell.

[0065] In embodiments of this application, the magnetic tunneling layer may include multiple film layers;

[0066] For example, the magnetic tunnel junction may include a reference layer, a barrier layer and a free layer. In this case, step S20 may include: sequentially forming a bottom electrode layer, a reference layer, a barrier layer, a free layer and a hard mask layer on the substrate.

[0067] For example, the magnetic tunnel junction may include a synthetic antiferromagnetic layer, a reference layer, a barrier layer and a free layer. In this case, step S20 may include: sequentially forming a bottom electrode layer, an antiferromagnetic layer, a reference layer, a barrier layer, a free layer and a hard mask layer on the substrate.

[0068] For example, the magnetic tunnel junction layer may include a synthetic antiferromagnetic layer, a ferromagnetic coupling layer, a reference layer, a barrier layer, and a free layer. In this case, step S20 may include: sequentially forming a bottom electrode layer, a synthetic antiferromagnetic layer, a ferromagnetic coupling layer, a reference layer, a barrier layer, a free layer, and a hard mask layer on the substrate.

[0069] In the embodiments of this application, the total thickness of the magnetic tunnel layer can be 10nm-20nm, and it has a bottom pinned structure.

[0070] In the embodiments of this application, the reference layer has magnetic polarization invariance, and the reference layer of a vertical MRAM (pSTT-MRAM) generally includes [Co / Ni].n Co / (Ru or Ir) / Co[Ni / Co] m [Co / Pd] n Co / (Ru or Ir) / Co[Pd / Co] m Or [Co / Pt] n Co / (Ru or Ir) / Co[Pt / Co] m The superlattice multilayer film structure has 0≤m≤3, 2≤n≤7, and can achieve ferromagnetic coupling with cobalt iron boron (CoFeB), cobalt ferrode (CoFe) / cobalt iron boron (CoFeB), cobalt ferrode (CoFe) / nickel iron alloy (NiFe), cobalt boron (CoB), or iron boron (FeB) through lattice isolation layers; the total thickness of the reference layer can be 4nm-15nm.

[0071] In the embodiments of this application, the material of the barrier layer can be a non-magnetic metal oxide, such as magnesium oxide (MgO), zinc magnesium oxide (MgZnO), boron magnesium oxide (MgBO), aluminum magnesium oxide (MgAlO), preferably magnesium oxide (MgO); the thickness of the barrier layer can be 0.5nm-2.5nm.

[0072] In the embodiments of this application, the free layer has variable magnetic polarization, and the material of the vertical pSTT-MRAM free layer can be cobalt iron boron (CoFeB), CoFe / cobalt iron boron (CoFeB), iron (Fe) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB); the thickness of the free layer can be 0.8nm-2.3nm.

[0073] The hard mask layer can serve as the top electrode layer for forming the top electrode. The material of the hard mask layer can be tantalum (Ta), tantalum nitride (TaN), or tantalum (Ta) / tantalum nitride (TaN) to obtain better etching profiles in halogen plasmas and higher etching selectivity during MTJ and BE etching; the thickness of the hard mask layer can be 20nm-100nm.

[0074] Alternatively, a sacrificial mask layer can be deposited on the hard mask layer, and the forming material can be selected from any one or more of silicon oxide (SiO2), silicon carbide (SiC), silicon oxynitride (SiON), silicon nitride (SiN), and silicon carbide nitride (SiCN).

[0075] In an embodiment of this application, step S30 may include: using a three-layer mask to complete the patterning definition of the magnetic tunnel junction layer and the reactive ion etching (RIE) of the hard mask layer, and using RIE and / or wet processes to remove residual polymer so that the pattern is transferred to the top of the magnetic tunnel junction layer.

[0076] In the embodiments of this application, the preparation method may further include: during and / or after step S40, using ion beam etching to trim the sidewalls of the magnetic tunnel junction to obtain the magnetic tunnel junction array, so as to eliminate the redeposition and etching damage caused by the etching in the previous step.

[0077] In the embodiments of this application, the ion source gas for ion beam etching can be selected from any one or more of neon, argon, krypton, and xenon.

[0078] In embodiments of this application, the preparation method may further include: after trimming the sidewalls of the magnetic tunnel junction, depositing an insulating layer around the magnetic tunnel junction and on the surfaces of the top and bottom electrodes to cover the magnetic tunnel junction, the top electrode, and the bottom electrode.

[0079] In the embodiments of this application, the material of the insulating layer may be selected from silicon nitride (SiN), silicon carbide (SiC), and silicon oxide (SiO). x ), silicon oxynitride (SiON) and silicon carbide (SiCN) are any one or more of these.

[0080] This application also provides a magnetic tunnel junction array, which can be obtained by the preparation method described above.

[0081] In the embodiments of this application, the diameter of the magnetic tunnel junction array can be Sub-80nm, Sub-70nm, Sub-60nm or Sub-50nm.

[0082] Example 1

[0083] The method for fabricating the magnetic tunnel junction array in this embodiment is as follows: Figure 6 As shown, it includes:

[0084] S10: Provides a surface-polished CMOS substrate 100 with non-copper (Cu) vias 120. The substrate 100, excluding the vias 120, is a dielectric 110. Figure 6 As shown in (a) in the middle;

[0085] S20: On one side surface of the CMOS substrate 100, a bottom electrode layer 210 (forming the bottom electrode, BE), a magnetic tunnel junction layer 220 (forming the magnetic tunnel junction, MTJ), and a hard mask layer 230 (which can form the top electrode, TE, also called the top electrode layer) are sequentially deposited, such as... Figure 6 As shown in (b) in the image;

[0086] The material forming the bottom electrode layer 210 is generally Ti or TiN, etc.; and after the bottom electrode layer 210 is deposited, a chemical mechanical planarization process is generally used to planarize the bottom electrode layer 210 to obtain the planarization requirements for fabricating MTJ cells.

[0087] The magnetic tunnel junction 220 includes multiple film layers with a total thickness of 10nm-20nm. It is a structure formed by sequentially stacking a reference layer, a barrier layer and a free layer, and has a bottom pinning structure.

[0088] The reference layer has magnetic polarization invariance, and the reference layer of a vertical MRAM (pSTT-MRAM) typically includes [Co / Ni]. n Co / (Ru or Ir) / Co[Ni / Co] m [Co / Pd] n Co / (Ru or Ir) / Co[Pd / Co] m Or [Co / Pt] n Co / (Ru or Ir) / Co[Pt / Co] m The superlattice multilayer film structure can achieve ferromagnetic coupling with cobalt iron boron (CoFeB), cobalt ferrode (CoFe) / cobalt iron boron (CoFeB), cobalt ferrode (CoFe) / nickel iron alloy (NiFe), cobalt boron (CoB) or iron boron (FeB) through lattice isolation layers, and its total thickness can be 4nm-15nm.

[0089] The barrier layer can be made of a non-magnetic metal oxide, preferably magnesium oxide (MgO), and its thickness can be 0.5 nm to 2.5 nm.

[0090] The free layer has variable magnetic polarization. The material of the vertical pSTT-MRAM free layer can be cobalt iron boron (CoFeB), CoFe / cobalt iron boron (CoFeB), iron (Fe) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / tungsten (W) / cobalt iron boron (CoFeB), cobalt iron boron (CoFeB) / molybdenum (Mo) / cobalt iron boron (CoFeB), and its thickness can be 0.8nm-2.3nm.

[0091] The thickness of the hard mask layer 230 can be 20nm-100nm, and the material can be tantalum (Ta), tantalum nitride (TaN), or tantalum (Ta) / tantalum nitride (TaN) in order to obtain better etching profiles in halogen plasma and higher etching selectivity when etching MTJ and its BE.

[0092] A sacrificial mask layer can be deposited on the hard mask layer 230, and the material of the sacrificial mask layer can be silicon oxide (SiO2). x Silicon carbide (SiC), silicon oxynitride (SiON), silicon nitride (SiN), or silicon carbide nitride (SiCN), etc.

[0093] S30: Graphically define the pattern of the magnetic tunnel junction 220 and transfer the pattern to the top of the magnetic tunnel junction 220;

[0094] In this process, a three-layer mask is used to complete the patterning definition of the magnetic tunnel junction layer 220 and the reactive ion etching (RIE) of the hard mask layer 230. The residual polymer is removed by RIE process and / or wet process so that the pattern is transferred to the top of the magnetic tunnel junction layer 220.

[0095] S40: The magnetic tunnel junction layer 220 and the bottom electrode layer 210 are etched using a synergistic etching scheme of cyano radicals and inert gas ions. Figure 6 As shown in (c);

[0096] Specifically, this may include: forming cyano radicals in a plasma, such as a plasma formed by a cyano radical precursor gas and an inert gas, chemically reacting the cyano radicals with the materials of the patterned magnetic tunnel junction layer 220 and the hard mask layer 230 and / or chemically modifying the materials of the patterned magnetic tunnel junction layer 220 and the hard mask layer 230 with cyano radicals, and forming inert gas ions from the ion source gas of the inert gas ions, and using the inert gas ions to remove the chemical reaction products and / or the chemically modified materials and / or the patterned magnetic tunnel junction layer 220 and the hard mask layer 230 that have not undergone chemical reaction and have not been chemically modified;

[0097] The precursor gas of the cyano radical can be selected from any one or more of HCN, (CN)2, CH3CN, CH4 / NH3, CH3OH / NH3 and CH3CH2OH / NH3;

[0098] The pressure during the chemical reaction and / or the chemical modification can be 0.3 mTorr-10 mTorr;

[0099] The ion source gas for the inert gas ions may include any one or more of neon, argon, krypton, and xenon, and may add any one or more of CO, CO2, N2, O2, and He as a carrier gas.

[0100] The total flow rate of the precursor gas of the cyano radical and the ion source gas of the inert gas ions can be 100 sccm-2000 sccm.

[0101] The power of the radio frequency source power that generates and sustains the plasma can be 100 watts to 3000 watts;

[0102] The frequency of the radio frequency power source can be 13.56MHz;

[0103] The RF bias power supply can provide ion acceleration voltages ranging from 30V to 1000V; and the ion acceleration voltage can be pulsed.

[0104] The frequency of the radio frequency bias power supply can be 13.56MHz, 2MHz or 400kHz;

[0105] S50: During and / or after step S40, the sidewalls of the magnetic tunnel junction are trimmed by ion beam etching to obtain the magnetic tunnel junction array.

[0106] The ion source gas used for ion beam etching can be selected from any one or more of neon, argon, krypton, and xenon.

[0107] S60: An insulating layer 240 is deposited around the magnetic tunnel junction 220' of the magnetic tunnel junction array, and the insulating layer 240 covers the top electrode 230' and the bottom electrode 210'. Figure 6 As shown in (d);

[0108] The insulating layer 240 can be made of silicon nitride (SiN) or silicon oxide (SiO). x Silicon carbide (SiC), silicon oxynitride (SiON), or silicon carbide nitride (SiCN), etc.

[0109] While the embodiments disclosed in this application are as described above, the content is merely for the purpose of facilitating understanding of this application and is not intended to limit this application. Any person skilled in the art to which this application pertains may make any modifications and changes in the form and details of the implementation without departing from the spirit and scope disclosed in this application; however, the scope of protection of this application shall still be determined by the scope defined in the appended claims.

Claims

1. A method for fabricating a magnetic tunnel junction array, characterized in that, include: S10: Provides a substrate; S20: A bottom electrode layer, a magnetic tunnel junction layer, and a hard mask layer are sequentially formed on the substrate; S30: Pattern the magnetic tunneling layer and the hard mask layer; S40: The precursor gas of cyano radicals is used to form cyano radicals in plasma. The cyano radicals are then chemically reacted with the materials of the patterned magnetic tunnel junction layer and hard mask layer, and / or the materials of the patterned magnetic tunnel junction layer and hard mask layer are chemically modified using the cyano radicals. The ion source gas of the inert gas ions is then converted into inert gas ions. The inert gas ions are accelerated using an RF bias power supply, and the accelerated inert gas ions are used to bombard the chemical reaction products and / or chemically modified materials and / or the patterned magnetic tunnel junction layer and hard mask layer materials that have not undergone chemical reaction and have not been chemically modified in order to remove these materials, thereby obtaining a magnetic tunnel junction array. The total flow rate of the precursor gas of the cyano radical and the ion source gas of the inert gas ions is 100 sccm-2000 sccm. The power of the radio frequency source power supply that generates and sustains the plasma is 100 watt to 3000 watts; the frequency of the radio frequency source power supply is 13.56 MHz. The ion acceleration voltage provided by the radio frequency bias power supply is 30V-1000V; the frequency of the radio frequency bias power supply is 13.56MHz, 2MHz or 400kHz.

2. The preparation method according to claim 1, wherein, The material of the magnetic tunnel layer includes any one or more of iron, cobalt, cobalt iron boron, nickel, tungsten, molybdenum, chromium, ruthenium, iridium, palladium, platinum, magnesium oxide, aluminum, zinc, titanium, and rhodium.

3. The preparation method according to claim 1, wherein, The material of the hard mask layer is selected from tantalum and tantalum nitride, or any one or more of them.

4. The preparation method according to claim 1, wherein, The precursor gas for the cyano radical is selected from any one or more of HCN, (CN)2, CH3CN, CH4 / NH3, CH3OH / NH3 and CH3CH2OH / NH3.

5. The preparation method according to any one of claims 1 to 4, wherein, The pressure during the chemical reaction and / or the chemical modification is 0.3 mTorr-10 mTorr.

6. The preparation method according to any one of claims 1 to 4, wherein, The ion source gas for the inert gas ions includes any one or more of neon, argon, krypton, and xenon. The ion source gas for the inert gas ions also includes a carrier gas, which is selected from any one or more of CO, CO2, N2, O2 and He.

7. The preparation method according to any one of claims 1 to 4, wherein, The frequency of the radio frequency bias power supply is 400kHz.

8. The preparation method according to any one of claims 1 to 4, wherein, Step S40 is performed in an inductively coupled plasma etching chamber.

9. The preparation method according to any one of claims 1 to 4, further comprising: During and / or after step S40, the sidewalls of the magnetic tunnel junction are trimmed by ion beam etching to obtain the magnetic tunnel junction array. The ion source gas used for ion beam etching is selected from any one or more of neon, argon, krypton, and xenon.

10. A magnetic tunnel junction array, characterized in that, Obtained by the preparation method according to any one of claims 1 to 9; The magnetic tunnel junctions of the magnetic tunnel junction array have diameters of sub-80nm, sub-70nm, sub-60nm, or sub-50nm.

Citation Information

Patent Citations

  • Method for manufacturing ultra-small magnetic random access memory array

    CN111490151A

  • Etch selectivity by introducing oxidants to noble gas during physical magnetic tunnel junction (MTJ) etching