Aluminum-containing silicon-based adsorbent, preparation method thereof, and application of the adsorbent in removing glyphosate from water

By doping aluminum into the mesoporous silica skeleton, an aluminum-containing silicon-based adsorbent with an Al-O-Si structure is formed, which solves the problems of poor glyphosate adsorption selectivity and low capacity in the existing technology and achieves efficient removal Glyphosate is found in water bodies, is non-toxic and environmentally friendly, and is suitable for large-scale production.

CN116571206BActive Publication Date: 2024-10-15HUBEI THREE GORGES LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310472082.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-15
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Existing adsorbents have problems with poor adsorption selectivity, low capacity and residual pollutants during the preparation process in removing glyphosate from water. In particular, pure silicon-based mesoporous materials have poor adsorption performance for glyphosate.

Method used

Aluminum-containing silicon-based adsorbents are used, and the metal element aluminum is doped into the amorphous mesoporous silica skeleton to form a uniformly distributed Al-O-Si structure, which improves the adsorption capacity and selectivity of the adsorbent, and uses hydrothermal crystals. The chemical process and roasting process form a mesoporous structure.

Benefits of technology

It provides an adsorbent with high selectivity and large adsorption capacity, which can effectively remove glyphosate in water, is non-toxic, will not cause secondary pollution to water, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116571206B_ABST
    Figure CN116571206B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of an aluminum-silicon-based adsorbent and application of the adsorbent in treating glyphosate wastewater, wherein the aluminum-silicon-based adsorbent has an amorphous mesoporous silica as a skeleton. The aluminum-silicon-based adsorbent provided by the present invention is non-toxic, does not cause secondary pollution to water bodies, has a moderate specific surface area, pore volume and pore diameter, has a large glyphosate adsorption capacity, and has broad application prospects in the field of treating glyphosate wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water, wastewater or sewage treatment by adsorption method, and specifically relates to an aluminum-silicon-based adsorbent, a preparation method thereof and application of the adsorbent in removing glyphosate in water. Background Art

[0002] Glyphosate is a pollutant that exists in natural water bodies. This organophosphorus herbicide is widely used in agricultural production, but it and its metabolites are potentially carcinogenic. Due to excessive use of glyphosate and its water solubility, these substances will enter the water body with soil seepage, damaging the ecological environment. The European Drinking Water Directive stipulates that the content of glyphosate in safe surface water shall not exceed 0.1μg / L. Therefore, simply and efficiently enriching and removing glyphosate from water bodies is an important measure to control water pollution.

[0003] At present, common treatment methods for glyphosate pollution control include biological method, physical method, chemical precipitation method and adsorption method. Adsorption has become a unique technology in the process of environmental governance and has been widely used in the treatment of wastewater and waste gas. Adsorption is one of the effective methods for treating industrial wastewater. It is a method of using adsorbents to adsorb one or several pollutants in wastewater in order to recover or remove them, thereby purifying the wastewater. At present, the adsorption method has been applied to the treatment of glyphosate production wastewater and has achieved good results.

[0004] Adsorbents that can be used for the treatment of glyphosate production wastewater include mesoporous silica, activated carbon, adsorption resins, etc. Although activated carbon has the advantages of low cost and can adsorb a variety of pollutants, its adsorption selectivity is poor and its glyphosate adsorption capacity is low. Adsorption resins can effectively adsorb various types of compounds with different chemical properties, have good selectivity for organic matter, excellent performance, and stable physical and chemical properties. However, resin adsorbents are usually not rigid and easy to break, and the porogens and other raw materials or solvents used in the preparation process are not completely removed and remain, which can easily cause secondary pollution. Mesoporous silica materials have the characteristics of excellent adsorption materials: orderly pore structure; single and controllable pore size distribution, and diverse mesopore shapes, which make them extremely important in the fields of adsorption separation and environmental protection. Pure silicon-based mesoporous materials have low chemical activity and poor adsorption performance for glyphosate. A common way to solve this problem is to modify mesoporous silica to increase its surface activity, improve adsorption performance and selectivity, and expand its application range. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an aluminum-silicon-based adsorbent, a preparation method thereof and the application of the adsorbent in removing glyphosate in water bodies in view of the above-mentioned deficiencies in the prior art. The aluminum-silicon-based adsorbent has a large adsorption capacity for glyphosate and good selectivity, and has good application prospects in the treatment of glyphosate wastewater.

[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0007] The invention discloses an aluminum-containing silicon-based adsorbent. The adsorbent uses amorphous mesoporous silica as a skeleton. Metallic element aluminum is doped after the amorphous mesoporous silica is synthesized. The metallic element aluminum is evenly distributed on the surface and inside of the skeleton.

[0008] According to the above scheme, the average pore size of the amorphous mesoporous silica is 6-20 nm, and the pore volume is 0.7-1.3 cm 3 / g, specific surface area is 350~500m 2 / g.

[0009] The present invention also includes a method for preparing the above-mentioned aluminum-containing silicon-based adsorbent, and the specific steps are as follows:

[0010] 1) Prepare a certain concentration ratio of hydroxyethyl cellulose solution and sodium metasilicate solution, add the sodium metasilicate solution to the stirred hydroxyethyl cellulose solution at 88-92°C, and stir while keeping warm. Use an acid solution to adjust the pH of the system to weak acidity. After fully reacting for 1-3 hours, react at 25°C for 16-24 hours. Stop stirring and age for 16-20 hours. Add the aluminum-containing solution while stirring, adjust the solution pH to 4-6 with a sodium hydroxide solution, and stir for 0.5-2 hours to obtain a reaction solution;

[0011] 2) placing the reaction solution obtained in step 1) in a hydrothermal reactor, centrifuging, washing, drying, grinding and calcining the solid product after the hydrothermal crystallization reaction to obtain a solid adsorbent named Al(x)-HECMS, wherein x represents the Al / Si molar ratio.

[0012] According to the above scheme, the mass concentration ratio of the hydroxyethyl cellulose solution and the sodium metasilicate solution in step 1) is 1:25-30.

[0013] According to the above scheme, the dropping speed of the sodium metasilicate solution in step 1) is 2.5-5 mL / min.

[0014] According to the above scheme, step 1) the heating and stirring temperature is 88~92℃.

[0015] According to the above scheme, the aluminum source in step 1) is one of AlCl3·8H2O, Al2(SO4)3, and Al2Na2O4, the concentration of the aluminum solution is 0.01~0.2mol / L, and the molar ratio of aluminum element in the aluminum source solution to silicon element in the sodium metasilicate aqueous solution is 0.1-1:1.

[0016] According to the above scheme, in step 1), the stirring time after adding the aluminum source solution is 30-60 minutes. Stirring makes the aluminum ions more evenly distributed in the gel solution and less likely to agglomerate.

[0017] According to the above scheme, the acid solution in step 1) is a 6.4-7.5% hydrochloric acid solution.

[0018] Following the above scheme, the concentration of the sodium hydroxide solution in step 1) is 1-2 mol / L.

[0019] According to the above scheme, the hydrothermal crystallization reaction temperature in step 2) is 85-95°C, and the hydrothermal crystallization reaction time is 16-40h.

[0020] According to the above scheme, the calcination process conditions in step 2) are: heating to 450-550°C at a rate of 2-5°C / min at room temperature and keeping the temperature for 6-10 hours. During the calcination process, the surfactant hydroxyethyl cellulose is removed by increasing the temperature, thereby forming a mesoporous structure.

[0021] The present invention also includes the use of the above aluminum-silicon-based adsorbent in removing glyphosate from water.

[0022] The present invention firstly adopts the sol-gel method to prepare mesoporous silica, and then utilizes the hydrothermal crystallization process to make aluminum atoms in situ replace silicon atoms in the mesoporous silica skeleton, thereby forming a uniformly distributed Al-O-Si structure. Because the chemical behavior of most aluminum compounds under acidic and alkaline conditions varies greatly, the pH of the synthesis system must be paid attention to during the aluminum doping process. After adjusting the pH value in the first step of the present invention, the sol has formed a mesoporous silica (HECMS) skeleton structure. After adding the aluminum source and stirring it thoroughly, the pH value of the solution changes. At this time, the acidity of the solution is enhanced, and the metallic aluminum is in the form of Al 3+ In the second step, the pH value of the system is adjusted to 4-6 with alkali solution. 3+ It is converted into Al(OH)3, and through the action of hydrothermal crystallization, aluminum is combined with the silicon skeleton to form Al-O-Si bonds, effectively doping aluminum into the pore walls and pore surface of mesoporous silica. Due to the doping of metallic aluminum, the coordination effect of metallic aluminum is utilized to increase the adsorption capacity of mesoporous materials for glyphosate.

[0023] The beneficial effects of the present invention are as follows: 1. The aluminum-silicon-based adsorbent provided by the present invention is non-toxic, does not cause secondary pollution to water bodies, has a moderate specific surface area, pore volume and pore diameter, has a large glyphosate adsorption capacity, and has broad application prospects in the field of pesticide-containing wastewater treatment. 2. The preparation method of the present invention has simple steps, and the raw materials are cheap and readily available, which is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Nitrogen adsorption-desorption isotherms and pore size distribution diagram of the adsorbent (aluminum-silicon molar ratio = 0.3:1) prepared in Example 1 of the present invention.

[0025] Figure 2 Nitrogen adsorption-desorption isotherms and pore size distribution diagram of the adsorbent prepared in Example 2 (aluminum-silicon molar ratio = 0.2:1).

[0026] Figure 3 Nitrogen adsorption-desorption isotherms and pore size distribution diagram of the adsorbent prepared in Example 3 (aluminum-silicon molar ratio = 0.1:1).

[0027] Figure 4 This is a graph showing the equilibrium adsorption performance of the adsorbent prepared in Example 1 for glyphosate solutions with different pH values ​​at 30°C.

[0028] Figure 5 This is a graph showing the equilibrium adsorption performance of the aluminum-doped adsorbent prepared in Example 1 for glyphosate solutions with different initial concentrations at 30°C.

[0029] Figure 6 This is the wide-angle X-ray diffraction pattern of the adsorbent prepared in Example 1.

[0030] Figure 7 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of HECMS prepared in Comparative Example 1.

[0031] Figure 8 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of Zr-HECMS prepared in Comparative Example 2.

[0032] Fig. 9 This is a diagram showing the equilibrium adsorption performance of Fe-HECMS prepared in Comparative Example 3 for glyphosate solutions with different pH values ​​at 30°C. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.

[0034] Example 1

[0035] An aluminum-silicon-based adsorbent (aluminum-silicon molar ratio = 0.3:1) is prepared by the following steps:

[0036] 1) Add 3 g of hydroxyethyl cellulose to 300 mL of water, heat to 90 ° C and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21 g of Na2SiO3·9H2O in 50 mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the dropwise addition, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2 h, cool to 25 ° C, continue stirring for 24 h, stop stirring, stand and age for 20 h, add 10 mL of 1.5 mol / L aluminum source solution (AlCl3·6H2O dissolved in water), stir for 30 min, and then adjust the pH value of the system to 5 with 2 mol / L NaOH solution to obtain a reaction solution;

[0037] 2) The reaction solution was placed in a hydrothermal reactor, and after a hydrothermal crystallization reaction at 100°C for 24 hours, it was centrifuged and washed several times at a centrifugal speed of 9000 rpm, and each centrifugal time was 10 minutes. It was then dried at 100°C for 24 hours, and the obtained solid was ground. Finally, the solid was calcined from room temperature at a rate of 2°C / min to 550°C for 6 hours to obtain an aluminum-silicon-based adsorbent Al(0.3)-HECMS.

[0038] Figure 1 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the aluminum-containing silicon-based adsorbent Al(0.3)-HECMS prepared in Example 1. It can be seen from the figure that the nitrogen adsorption-desorption curve of the aluminum-doped HECMS material prepared in Example 1 is a type IV isotherm, which is the adsorption characteristic curve of the mesoporous material, indicating that the material has a mesoporous structure. The nitrogen adsorption-desorption curve shows an H2-type hysteresis loop, indicating that the pore structure is similar to that of an ink bottle. According to the nitrogen physical adsorption-desorption data, the specific surface area of ​​the material is 428.57 m 2 / g, pore volume 0.44cm 3 / g, with an average pore diameter of 4.17 nm, and has good properties of mesoporous materials.

[0039] Example 2

[0040] An aluminum-silicon-based adsorbent (aluminum-silicon molar ratio = 0.2:1) is prepared by the following steps:

[0041] 1) Add 3g of hydroxyethyl cellulose to 300mL of water, heat to 90℃ and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21g of Na2SiO3·9H2O in 50mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the dropwise addition, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2h, cool to 25℃, continue stirring for 24h, stop stirring, stand and age for 20h, add 10mL of 1mol / L aluminum source solution (dissolved in water to obtain AlCl3·6H2O), stir for 30min, and then adjust the pH value of the system to 5 with 2mol / L NaOH solution to obtain a reaction solution;

[0042] 2) The reaction solution was placed in a hydrothermal reactor, and after a hydrothermal crystallization reaction at 100°C for 24 hours, it was centrifuged and washed several times at a centrifugal speed of 9000 rpm, and each centrifugal time was 10 minutes. It was then dried at 100°C for 24 hours, and the obtained solid was ground. Finally, the solid was calcined from room temperature at a rate of 2°C / min to 550°C for 6 hours to obtain an aluminum-silicon-based adsorbent Al(0.2)-HECMS.

[0043] Figure 2 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the aluminum-containing silicon-based adsorbent Al(0.2)-HECMS prepared in Example 2. According to the nitrogen physical adsorption-desorption data, the specific surface area of ​​the aluminum-containing silicon-based adsorbent prepared in this example is 456.96 m 2 / g, pore volume 0.59cm 3 / g, and the average pore size is 4.97 nm.

[0044] Example 3

[0045] An aluminum-silicon-based adsorbent (aluminum-silicon molar ratio = 0.1:1) is prepared by the following steps:

[0046] 1) Add 3 g of hydroxyethyl cellulose to 300 mL of water, heat to 90 ° C and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21 g of Na2SiO3·9H2O in 50 mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the dropwise addition, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2 h, cool to 25 ° C, continue stirring for 24 h, stop stirring, stand and age for 20 h, add 10 mL of 0.5 mol / L aluminum source solution (AlCl3·6H2O dissolved in water), stir for 30 min, and then adjust the pH value of the system to 5 with 2 mol / L NaOH solution to obtain a reaction solution;

[0047] 2) The reaction solution was placed in a hydrothermal reactor, and after a hydrothermal crystallization reaction at 100°C for 24 hours, it was centrifuged and washed several times at a centrifugal speed of 9000 rpm, and each centrifugal time was 10 minutes. It was then dried at 100°C for 24 hours, and the obtained solid was ground. Finally, the solid was calcined from room temperature at a rate of 2°C / min to 550°C for 6 hours to obtain an aluminum-silicon-based adsorbent Al(0.1)-HECMS.

[0048] Figure 3 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the aluminum-containing silicon-based adsorbent Al(0.1)-HECMS prepared in Example 3. According to the nitrogen physical adsorption-desorption data, the specific surface area of ​​the aluminum-containing silicon-based adsorbent prepared in this example is 530.12 m 2 / g, pore volume 0.81cm 3 / g, and the average pore size is 6.12nm.

[0049] Figure 4 The following is the equilibrium adsorption curve of the aluminum-silicon-based adsorbent Al(0.3)-HECMS prepared in Example 1 for glyphosate solutions with different pH values ​​at 30°C. Take multiple portions of glyphosate solution with a concentration of 100 mg / L, 50 mL each, and adjust the pH values ​​to 2, 3, 4, 5, 6, 7, 8, 9, 10, and 11 respectively. Add 0.05 g of the Al(0.3)-HECMS adsorbent prepared in Example 1 to each portion of glyphosate solution. Adsorb for 24 hours at a temperature of 30°C to test the adsorption effect of the aluminum-silicon-based adsorbent on glyphosate (each sample was repeated three times and the average value was taken). The results show that when the pH value of the solution is 3.0, the adsorption amount of glyphosate by the adsorbent is the largest, reaching 83.16 mg / g. At pH values ​​of 3-11, the adsorption amount decreases rapidly with the increase of the pH value of the solution.

[0050] Figure 5The following is the equilibrium adsorption curve of Al(0.3)-HECMS prepared in Example 1 for glyphosate solutions of different initial concentrations at 30°C. Take multiple glyphosate solutions of different concentrations (concentration 25-300 mg / L), each 50 mL, adjust the pH value to 3, add 0.05g of the adsorbent prepared in Example 1 to each glyphosate solution, adsorb for 24h at a temperature of 30°C, and test the adsorption effect of Al(0.3)-HECMS on glyphosate solutions of different concentrations. It can be seen that as the initial concentration of the glyphosate solution increases, the equilibrium adsorption amount of glyphosate by Al(0.3)-HECMS increases. When the initial concentration of glyphosate is greater than 250 mg / L, the equilibrium adsorption amount does not change much with the increase in concentration. This is because when the initial concentration of glyphosate is greater than 250 mg / L, the adsorption active sites are gradually occupied by glyphosate, and the adsorption reaches saturation. The adsorption amount is the highest at C0=300 mg / L, reaching 182.90 mg / g.

[0051] Figure 6 XRD patterns of the HECMS adsorbent prepared in Comparative Example 1 and the aluminum-containing silicon-based adsorbent Al(0.3)-HECMS prepared in Example 1. Both samples showed characteristic diffraction peaks of silica near 2θ=23°. The XRD pattern after Al doping did not change, indicating that Al ions were highly dispersed in mesoporous silica.

[0052] Comparative Example 1

[0053] A mesoporous silica adsorbent (HECMS) free of aluminum is prepared by the following steps:

[0054] 1) Add 3 g of hydroxyethyl cellulose to 300 mL of water, heat to 90 °C and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21 g of Na2SiO3·9H2O in 50 mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the dropwise addition, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2 h, cool to 25 °C, continue stirring for 24 h, stop stirring, and let stand for 20 h to obtain a reaction solution;

[0055] 2) The reaction solution was washed by centrifugation for multiple times at a centrifugal speed of 9000 rpm for 10 min, and then dried at 100 °C for 12 h. The obtained solid was ground and finally calcined at a rate of 2 °C / min from room temperature to 550 °C for 6 h to obtain a solid adsorbent HECMS.

[0056] Figure 7The nitrogen adsorption-desorption isotherm and pore size distribution diagram of HECMS prepared in this comparative example 1. As can be seen from the figure, the nitrogen adsorption-desorption curve of HECMS material is a type IV isotherm, and the nitrogen adsorption-desorption curve shows an H2 type hysteresis loop, indicating that Al(0.3)-HECMS has a mesoporous structure similar to that of HECMS. After testing, the specific surface area of ​​the adsorbent prepared in this comparative example is 525.44 m 2 / g, pore volume 0.47 cm 3 / g, and the average pore size is 3.59 nm.

[0057] Take 2 portions of 100 mg / L glyphosate solution, 50 mL each, adjust the pH value to 3, add 0.05 g of HECMS prepared in this comparative example 1 to each portion of glyphosate solution, adsorb at a temperature of 30°C for 24 hours, and test the adsorption effect of HECMS on glyphosate. Taking the average value of the test results, the adsorption amount of glyphosate by HECMS was measured to be 2.65 mg / g. Under the same conditions, the adsorption amount of glyphosate by Al(0.3)-HECMS prepared in Example 1 reached 83.16 mg / g. It shows that the aluminum-doped modified HECMS in Example 1 greatly improves the adsorption performance of the adsorbent for glyphosate.

[0058] Comparative Example 2

[0059] A zirconium-containing silicon-based adsorbent, the preparation method thereof has the following steps:

[0060] 1) Add 3 g of hydroxyethyl cellulose (viscosity 250-450 mpa·s, 25°C) to 300 mL of water, heat to 90°C and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21 g of Na2SiO3·9H2O in 50 mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the addition process, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2 h, cool to 25°C, continue stirring for 24 h, stop stirring, stand and age for 20 h, add 15 mL of 1.67 mol / L zirconium salt solution (ZrOCl2·8H2O dissolved in water), stir for 30 min, and then adjust the pH value of the system to 5 with 2 mol / L NaOH solution to obtain reaction solution A;

[0061] 2) The reaction solution A was placed in a hydrothermal reactor, and after a hydrothermal crystallization reaction at 100°C for 24 hours, it was centrifuged and washed several times at a centrifugal rate of 9000 rpm and a centrifugal time of 10 minutes each time, and then dried at 100°C for 24 hours, and the obtained solid was ground. Finally, the solid was calcined, and the temperature was raised from room temperature to 550°C at a rate of 2°C / min, and kept warm for 6 hours, and the solid adsorbent Zr-HECMS was collected.

[0062] Figure 8 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of Zr-HECMS prepared in this comparative example 2. After testing, the specific surface area of ​​the adsorbent prepared in this comparative example 2 is 258.62 m 2 / g, pore volume 0.71cm 3 / g, the average pore size is 10.92nm. Take 2 portions of 100 mg / L glyphosate solution, each 50 mL, adjust the pH value to 3, add 0.05 g of Zr-HMS prepared in this comparative example 1 to each portion of glyphosate solution, adsorb at a temperature of 30°C for 24h, and test the adsorption effect of Zr-HMS on glyphosate. Take the average value of the test results, and the adsorption amount of glyphosate is measured to be 30.36 mg / g.

[0063] Comparative Example 3

[0064] An iron-containing silicon-based adsorbent, the preparation method thereof has the following steps:

[0065] 1) Add 3 g of hydroxyethyl cellulose to 300 mL of water, heat to 90 °C and stir to dissolve to obtain a hydroxyethyl cellulose solution, dissolve 14.21 g of Na2SiO3·9H2O in 50 mL of water to obtain a sodium metasilicate solution, then drop the sodium metasilicate solution into the hydroxyethyl cellulose solution, keep the temperature constant during the dropwise addition, stir for 30 min, then adjust the pH value of the system to 5-6 with 2 mol / L hydrochloric acid solution, stir for 2 h, cool to 25 °C, continue stirring for 24 h, stop stirring, and let stand for 20 h to obtain a reaction solution;

[0066] 2) The reaction solution was centrifuged and washed several times at a centrifugal speed of 9000rpm for 10min, then dried at 100℃ for 12h, and the obtained solid was ground. Finally, the solid was calcined, and the temperature was raised from room temperature to 550℃ at a rate of 2℃ / min for 6h to obtain the solid adsorbent HECMS. Weigh 0.84g of ferric chloride hexahydrate (FeCl3·6H2O) and dissolve it in 50mL of water. 1.0g of HECMS was added to the solution, mixed and stirred for 24h, evaporated at 80℃, and calcined at 550℃ for 4h in a muffle furnace (heating rate of 2℃ / min) to obtain metallic iron-modified mesoporous silica, which was named Fe-HECMS.

[0067] After testing, the specific surface area of ​​the adsorbent prepared in this comparative example 3 is 203.98m 2 / g, pore volume 0.57cm 3 / g, and the average pore size is 10.68nm.

[0068] Fig. 9The following is the equilibrium adsorption curve of the iron-containing silicon-based adsorbent Fe-HECMS prepared in Comparative Example 3 for glyphosate solutions with different pH values ​​at 30°C. Take multiple portions of glyphosate solution with a concentration of 100 mg / L, 50 mL each, and adjust the pH values ​​to 2, 3, 4, 5, 6, 7, 8, and 9 respectively. Add 0.05 g of the Fe-HECMS adsorbent prepared in Example 1 to each portion of the glyphosate solution. Adsorb for 24 hours at a temperature of 30°C to test the adsorption effect of the iron-containing silicon-based adsorbent on glyphosate (each sample was repeated three times and the average value was taken). The results show that when the pH value of the solution is 3.0, the Fe-HECMS adsorbent has the largest adsorption amount of glyphosate, which can reach 11.62 mg / g.

Claims

1. An aluminum-silicon-based adsorbent, characterized in that: The adsorbent has amorphous mesoporous silica as a skeleton, and the metal element aluminum is doped after the amorphous mesoporous silica is synthesized, and the metal element aluminum is evenly distributed on the surface and inside of the skeleton. The specific steps are as follows: 1) Prepare a hydroxyethyl cellulose solution and a sodium metasilicate solution with a certain concentration ratio, add the sodium metasilicate solution to the stirred hydroxyethyl cellulose solution at 88-92°C, keep warm and stir, adjust the pH of the system to 5-6 with an acid solution, react for 1-3 hours, react at 25°C for 16-24 hours, stop stirring, age for 16-20 hours, add an aluminum solution while stirring, adjust the pH of the solution to 4-6 with a sodium hydroxide solution, stir for 0.5-2 hours to obtain a reaction solution, and the molar ratio of aluminum element in the aluminum salt solution to silicon element in the sodium metasilicate aqueous solution is 0.1-1:1; 2) placing the reaction solution obtained in step 1) in a hydrothermal reactor, centrifuging, washing, drying, grinding and calcining the solid product after the hydrothermal crystallization reaction to obtain a solid adsorbent, the hydrothermal crystallization reaction temperature is 85-95° C., and the hydrothermal crystallization reaction time is 16-40 h.

2. The aluminum-containing silicon-based adsorbent according to claim 1, characterized in that The amorphous mesoporous silica has an average pore diameter of 6 to 20 nm and a pore volume of 0.7 to 1.3 cm 3 / g, specific surface area is 350~500m 2 / g.

3. A method for preparing the aluminum-silicon-based adsorbent according to claim 1 or 2, characterized in that: The specific steps are as follows: 1) Prepare a hydroxyethyl cellulose solution and a sodium metasilicate solution with a certain concentration ratio, add the sodium metasilicate solution to the stirred hydroxyethyl cellulose solution at 88-92°C, keep warm and stir, adjust the pH of the system to 5-6 with an acid solution, react for 1-3 hours, react at 25°C for 16-24 hours, stop stirring, age for 16-20 hours, add the aluminum-containing solution while stirring, adjust the pH of the solution to 4-6 with a sodium hydroxide solution, and stir for 0.5-2 hours to obtain a reaction solution; 2) placing the reaction solution obtained in step 1) in a hydrothermal reactor, centrifuging, washing, drying, grinding and calcining the solid product after the hydrothermal crystallization reaction to obtain a solid adsorbent.

4. The method for preparing the aluminum-containing silicon-based adsorbent according to claim 3, characterized in that: Step 1) The mass concentration ratio of the hydroxyethyl cellulose solution to the sodium metasilicate solution is 1:25-30, and the dropping speed of the sodium metasilicate solution is 2.5-5 mL / min.

5. The method for preparing the aluminum-silicon-based adsorbent according to claim 3, characterized in that: Step 1) The heating and stirring temperature is 88~92℃.

6. The method for preparing the aluminum-silicon-based adsorbent according to claim 3, characterized in that: Step 1) the aluminum source is one of AlCl3·8H2O, Al2(SO4)3, and Al2Na2O4, the concentration of the aluminum solution is 0.01-0.2 mol / L, and the molar ratio of aluminum element in the aluminum salt solution to silicon element in the sodium metasilicate aqueous solution is 0.1-1:1; The stirring time after adding the aluminum source solution is 30-60 minutes.

7. The method for preparing the aluminum-containing silicon-based adsorbent according to claim 3, characterized in that: Step 1) The acid solution is a 6.4-7.5% hydrochloric acid solution; the concentration of the sodium hydroxide solution is 1-2 mol / L.

8. The method for preparing an aluminum-silicon-based adsorbent according to claim 3, characterized in that: Step 2) The hydrothermal crystallization reaction temperature is 85-95° C., and the hydrothermal crystallization reaction time is 16-40 hours.

9. The method for preparing an aluminum-silicon-based adsorbent according to claim 3, characterized in that: Step 2) The calcination process conditions are: heating to 450-550°C at a heating rate of 2-5°C / min at room temperature and keeping the temperature for 6-10 hours.

10. Use of the aluminum-silicon-based adsorbent according to claim 1 or 2 in removing glyphosate from water.