Method and apparatus for producing metallized pellets
By optimizing the mixing and molding of iron ore powder, reducing coal, and binder, as well as heat recovery and utilization, the problems of high raw material grade and high energy consumption in traditional direct reduction ironmaking technology have been solved. This has resulted in the production of efficient and low-cost metallized pellets suitable for blast furnace smelting, thereby reducing energy consumption and CO2 emissions in blast furnace ironmaking.
Patent Information
- Application Number
- CN202310540632.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Traditional direct reduction ironmaking technology requires high-grade raw materials and suffers from low reduction rates and high energy consumption, making it difficult to meet the requirements of blast furnace production for burden strength and efficiency.
Metallized pellets are produced by mixing iron ore powder, reducing coal, and binder, followed by molding, drying and preheating with a chain grate machine, calcining in a rotary kiln, and cooling with an annular cooler. This process optimizes equipment connections and heat recovery, thereby improving reduction efficiency and product quality.
The produced metallized pellets meet the compressive strength, drop strength, and drum strength requirements for use in large blast furnaces, reducing blast furnace ironmaking costs, increasing output, and reducing CO2 emissions, thus providing economic and ecological benefits.
Smart Images

Figure CN116574899B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of low-carbon ironmaking production technology, and in particular relates to a method and apparatus for producing metallized pellets. Background Technology
[0002] Traditional steel production relies heavily on long processes involving blast furnaces and converters, resulting in lengthy processes, high energy consumption, and significant pollutant emissions. Using low-carbon furnace charges is a primary means of reducing energy consumption, CO2 emissions, and improving production efficiency in ironmaking, and it has been widely adopted both domestically and internationally. Low-carbon furnace charges include scrap steel, direct reduced iron (DRI), carbon-containing pellets, and coke. Scrap steel is used in the largest quantity, but its irregular shape affects blast furnace charging. Carbon-containing pellets and coke do not meet the strength requirements of blast furnace charges. Direct reduced iron, with its regular shape and high strength at both room and high temperatures, has the potential for large-scale application in blast furnace ironmaking.
[0003] Currently, traditional direct reduction ironmaking technologies mainly include two types: gas-based vertical shaft furnace direct reduction and coal-based rotary kiln direct reduction ironmaking. The produced direct reduced iron is mainly used in blast furnaces. However, traditional direct reduction ironmaking technologies have high requirements for raw material grade, which is difficult to reconcile with the decreasing reserves of high-grade iron ore. Therefore, developing a method to produce high-strength metallized pellets from low-grade ore for blast furnace smelting has become a key focus of the industry. Due to the characteristics of my country's energy structure, it is difficult to promote the large-scale use of gas-based vertical shaft furnace direct reduction ironmaking technology. However, my country has abundant coal resources, which allows for the vigorous development of coal-based rotary kiln direct reduction ironmaking technology. Traditional coal-based direct reduction ironmaking technology uses oxidized pellets as raw materials. Metallized pellets are prepared by reducing oxidized pellets in a rotary kiln using reducing gas generated from the cracking and incomplete combustion of reducing coal. This method suffers from low reduction rate and high energy consumption. Therefore, it is necessary to develop a metallized pellet production method with high production efficiency, low energy consumption, and product quality that meets the requirements of blast furnace production. Summary of the Invention
[0004] In order to overcome the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a method and apparatus for producing metallized pellets, the products of which can reduce the blast furnace coke ratio, increase blast furnace output, reduce CO2 emissions from blast furnace ironmaking and reduce ironmaking production costs when used in blast furnace smelting.
[0005] The specific technical solution of this invention is as follows:
[0006] This invention provides a method for producing metallized pellets, the method comprising the following steps:
[0007] S1. Iron ore powder, reducing coal, binder and water are mixed in a predetermined mass ratio, and the mixture is pressure molded to obtain carbon-containing pellets.
[0008] S2. The carbon-containing pellets are dried and preheated on a chain grate machine to obtain preheated carbon-containing pellets. The chain grate machine includes a drying section and a preheating section connected in sequence.
[0009] S3. The preheated carbon-containing pellets are calcined in a rotary kiln to prepare metallized pellets by self-reduction. The rotary kiln includes a high-temperature calcination section and a cooling section, which are connected.
[0010] S4. The metallized pellets are cooled in an annular cooler to obtain the metallized pellet product. The annular cooler includes multiple cooling sections connected in sequence with different cooling temperatures.
[0011] In a preferred embodiment, the sequentially connected drying section and preheating section include a first drying section, a second drying section, a first preheating section, and a second preheating section connected in sequence.
[0012] The plurality of sequentially connected cooling sections include a first cooling section, a second cooling section, and a third cooling section connected in sequence.
[0013] The predetermined mass ratio is 65%-80% iron ore powder, 8%-16% reducing coal, 2%-10% binder, and 5%-15% moisture.
[0014] In a preferred embodiment, the flue gas generated by the rotary kiln is conveyed to the preheating stage, and the flue gas from the preheating stage is conveyed to the drying stage.
[0015] In a preferred embodiment, the exhaust gas generated in the first cooling stage is sent to the first preheating stage, and the exhaust gas generated in the second cooling stage is sent to the first drying stage.
[0016] In a preferred embodiment, the iron ore powder is any one or a mixture of several of hematite, magnetite, limonite, and vanadium-titanium magnetite.
[0017] In a preferred embodiment, the reducing coal includes any one or a mixture of several of anthracite, lean coal, semi-coke powder, and coke powder.
[0018] In a preferred embodiment, the adhesive is any one or a mixture of two of organic and inorganic adhesives.
[0019] In a preferred embodiment, the iron ore powder, reducing coal, and binder have a particle size of less than 0.1 mm.
[0020] In a preferred embodiment, in step S1, the molding pressure for pressure molding the mixed material is 10MPa-50MPa, and the carbon-containing pellets have a drop strength of more than 5 times at a depth of 0.5m.
[0021] In a preferred embodiment, the flue gas temperature in the first drying stage is less than 200°C and the oxygen content is less than 10%; the flue gas temperature in the second drying stage is less than 300°C and the oxygen content is less than 7%; the flue gas temperature in the first preheating stage is less than 400°C and the oxygen content is less than 4%; the flue gas temperature in the second preheating stage is less than 700°C and the oxygen content is less than 2%; and the total drying and preheating time of the carbon-containing pellets in the chain grate machine is 20-60 minutes.
[0022] In a preferred embodiment, in step S2, the temperature of the preheated carbon-containing pellets is greater than 300°C, and the 0.5m drop strength of the preheated carbon-containing pellets is greater than 10 times.
[0023] In a preferred embodiment, in step S3, the calcination and reduction temperature of the rotary kiln is 1150℃-1300℃, and the calcination and reduction time is 30-180min.
[0024] In a preferred embodiment, in step S3, the metallized pellets calcined in the rotary kiln need to be cooled in a cooling shaft furnace. The cooling gas is any one or a mixture of several of nitrogen, hydrogen, carbon monoxide, and methane. After cooling, the temperature of the metallized pellets is less than 900°C.
[0025] In a preferred embodiment, the first-stage metallized pellet is cooled to a temperature below 700°C, the second-stage metallized pellet is cooled to a temperature below 400°C, and the third-stage metallized pellet is cooled to a temperature below 100°C.
[0026] In a preferred embodiment, the annular cooler is cooled by gas, and the gas is exhaust gas with an oxygen content of less than 1%.
[0027] In a preferred embodiment, in step S4, the cooled metallized pellets have a metallization rate greater than 65%, a compressive strength greater than 2000 N / pellet, a 2m drop strength greater than 10 times, a drum strength greater than 90%, and an abrasion resistance index less than 5%.
[0028] In addition, this application also provides an apparatus for producing metallized pellets, comprising:
[0029] The silos are used to hold iron ore powder, reducing coal, and binder respectively.
[0030] The mixing machine is used to mix the iron ore powder, reducing coal, and binder after they are fed from the hopper to form a homogenized mixture.
[0031] A briquetting machine, connected to the mixer, is used to press the mixed material into carbon-containing green briquettes.
[0032] A chain grate machine, connected to the briquetting machine, is used to dry and preheat the carbon-containing raw pellets on the chain grate machine. The chain grate machine includes a drying section and a preheating section connected in sequence.
[0033] A rotary kiln, which is connected to the preheating section of the chain grate machine, the rotary kiln including a high-temperature roasting section and a cooling section;
[0034] A cooling vertical furnace, wherein the cooling section is connected to the cooling vertical furnace;
[0035] An annular cooler is connected to the cooling vertical furnace, and the annular cooler includes multiple cooling sections connected in sequence with different cooling temperatures.
[0036] In a preferred embodiment, the sequentially connected drying section and preheating section include a first drying section, a second drying section, a first preheating section, and a second preheating section connected in sequence.
[0037] The plurality of sequentially connected cooling sections include a first cooling section, a second cooling section, and a third cooling section connected in sequence.
[0038] In a preferred embodiment, the rotary kiln is connected to the second preheating stage via a flue gas duct, and the second preheating stage is connected to the second drying stage via a regenerating fan.
[0039] In a preferred embodiment, the first cooling stage is connected to the first preheating stage via a preheating fan, and the second cooling stage is connected to the first drying stage via a drying fan.
[0040] The beneficial effects of this application, based on the above technical solutions, are as follows:
[0041] 1. The method and apparatus for producing metallized pellets of the present invention are simple in equipment, convenient in operation, and have a wide range of applications. Compared with the traditional coal-based rotary kiln direct reduction technology, it overcomes the disadvantages of low production efficiency, complex process and narrow range of application.
[0042] 2. The method and apparatus for producing metallized pellets of the present invention achieve efficient preheating and reduction of carbon-containing pellets, and have the characteristics of low equipment investment, high production efficiency and excellent product quality. The compressive strength, drop strength and drum strength of the produced metallized pellets meet the requirements of large blast furnaces.
[0043] 3. This invention uses low-quality iron ore powder and reducing coal to produce metallized pellets, replacing sintered ore and pellets as blast furnace feedstock. This can reduce blast furnace ironmaking costs, increase output, reduce coke ratio and reduce CO2 emissions, resulting in significant economic, social and ecological benefits.
[0044] Specific embodiments of this application are disclosed in detail with reference to the following description and accompanying drawings, indicating how the principles of this application can be adopted. It should be understood that the embodiments of this application are not limited in scope. Within the spirit and scope of the appended claims, embodiments of this application include many changes, modifications, and equivalents.
[0045] Features described and / or illustrated for one embodiment may be used in the same or similar manner in one or more other embodiments, combined with features in other embodiments, or substituted for features in other embodiments.
[0046] It should be emphasized that the term "including / comprises" as used herein refers to the presence of a feature, whole, step, or component, but does not exclude the presence or addition of one or more other features, wholes, steps, or components. Attached Figure Description
[0047] The accompanying drawings described herein are for illustrative purposes only and are not intended to limit the scope of this application in any way. Furthermore, the shapes and scales of the components in the drawings are merely illustrative to aid in understanding this application and do not specifically limit the shapes and scales of the components. Those skilled in the art, guided by the teachings of this application, can select various possible shapes and scales to implement this application according to specific circumstances. In the drawings:
[0048] Figure 1 This is a flowchart illustrating a method for producing metallized pellets according to an embodiment of this application.
[0049] Figure 2 This is a diagram of an apparatus for producing metallized pellets according to an embodiment of this application.
[0050] The reference numerals in the above figures are as follows:
[0051] A. Reduced coal, B. Iron ore powder, C. Binder, D. Mixed material, E. Blended material, F. Carbon-containing green pellets, G. Metallized pellets, H. Rotary kiln fuel, I. Primary combustion air, J. Secondary combustion air, K. Cooling gas, L. Purified exhaust gas-I, M. Purified exhaust gas-II, N. Purified exhaust gas-III, O. Exhaust gas;
[0052] 1. Material hopper, 2. Conveying belt, 3. Mixer, 4. Briquetting machine, 5. Chain grate machine, 51. Drying section 1, 52. Drying section 2, 53. Preheating section 1, 54. Preheating section 2, 55. Regenerating fan, 56. Blowing fan, 57. Main exhaust fan, 58. Preheating fan, 6. Rotary kiln, 61. High-temperature roasting section, 62. Rotary kiln cooling section, 63. Burner, 64. Cooling shaft furnace, 65. Combustion lance, 7. Circular cooler, 71. Cooling section 1, 72. Cooling section 2, 73. Cooling section 3, 74. Cooling section 1 fan, 75. Cooling section 2 fan, 76. Cooling section 3 fan. Detailed Implementation
[0053] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0054] It should be noted that when an element is referred to as being "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only possible implementation.
[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0056] like Figure 1 As shown, the present invention provides a method for producing metallized pellets, comprising the following steps:
[0057] S1. Iron ore powder B, reducing coal A, binder C and water are mixed in a predetermined mass ratio, and the mixture E is pressure molded to obtain carbon-containing pellets.
[0058] S2. The carbon-containing green pellets are dried and preheated on a chain grate machine to obtain preheated carbon-containing pellets. The chain grate machine includes a drying section and a preheating section connected in sequence. Preferably, the chain grate machine is composed of a drying section 1, a drying section 2, a preheating section 1, and a preheating section 2 connected in sequence. This configuration can improve production efficiency and product quality while simplifying equipment, reducing costs, achieving efficient preheating of carbon-containing pellets, low equipment investment, high production efficiency, and excellent product quality. The compressive strength, drop strength, and drum strength of the produced metallized pellets meet the requirements for use in large blast furnaces.
[0059] S3. The preheated carbon-containing pellets are roasted in a rotary kiln to produce metallized pellets through self-reduction. The rotary kiln consists of a high-temperature roasting section and a cooling section, which can achieve efficient reduction of carbon-containing pellets. The equipment investment is low, the production efficiency is high, and the product quality is excellent. The compressive strength, drop strength, and drum strength of the produced metallized pellets meet the requirements for use in large blast furnaces.
[0060] S4. The metallized pellets are cooled in an annular cooler to obtain metallized pellet products that meet the requirements. The annular cooler includes multiple cooling sections connected in sequence with different cooling temperatures. Preferably, the annular cooler is composed of a first cooling section, a second cooling section, and a third cooling section connected in sequence with different cooling temperatures. This configuration can improve cooling efficiency and product quality while simplifying equipment, reducing costs, achieving efficient cooling of carbon-containing pellets, low equipment investment, high production efficiency, and excellent product quality. The compressive strength, drop strength, and drum strength of the produced metallized pellets meet the requirements for use in large blast furnaces.
[0061] Please see the appendix Figure 2 In step S1, the pulverized reducing coal A, iron ore powder B, and binder C are stored in their respective silos 1, and then mixed into a mixture D according to a predetermined mass ratio via the discharge ports of the corresponding silos 1 and a weighing device (not shown in the figure). The predetermined mass ratio is: iron ore powder B at 65%-80% mass percentage, reducing coal A at 8%-16% mass percentage, binder C at 2%-10% mass percentage, and moisture at 5%-15% mass percentage. Iron ore powder B is any one or a mixture of hematite, magnetite, limonite, and vanadium-titanium magnetite. Reducing coal A includes any one or a mixture of anthracite, lean coal, semi-coke powder, and coke powder. Binder C is any one or a mixture of two organic and inorganic binders. The particle size of iron ore powder B, reducing coal A, and binder C is all less than 0.1 mm.
[0062] Then, the mixture D is conveyed to the mixer 3 via the conveyor belt 2, where water is added and mixed to form a homogenized material E. Next, the homogenized material E is conveyed to the briquetting machine 4 for briquetting to obtain carbon-containing green pellets F. The molding pressure of the homogenized material E is 10MPa-50MPa, and the carbon-containing green pellets F have a drop strength of more than 5 times at 0.5m.
[0063] In step S2, the carbon-containing green pellets F are transported to the chain grate machine 5 and subjected to drying and preheating through a first drying stage 51, a second drying stage 52, a first preheating stage 53, and a second preheating stage 54. Specifically, the flue gas temperature in the first drying stage 51 is less than 200℃ and the oxygen content is less than 10%; the flue gas temperature in the second drying stage 52 is less than 300℃ and the oxygen content is less than 7%; the flue gas temperature in the first preheating stage 53 is less than 400℃ and the oxygen content is less than 4%; and the flue gas temperature in the second preheating stage 54 is less than 700℃ and the oxygen content is less than 2%. The total drying and preheating time for the carbon-containing pellets in the chain grate machine 5 is 20-60 minutes. The temperature of the preheated carbon-containing pellets is greater than 300℃, and the drop strength of the preheated carbon-containing pellets from 0.5m is greater than 10 times.
[0064] In step S3, the preheated carbon-containing pellets are placed in rotary kiln 6 and calcined and reduced in the high-temperature calcination section 61 of rotary kiln 6. The calcination and reduction temperature of rotary kiln 6 is 1150℃-1300℃, and the calcination and reduction time is 30-180 min. After calcination and reduction, the carbon-containing pellets are cooled in the cooling section 62 of rotary kiln, and then discharged into the cooling shaft furnace 64 to exchange heat with the cooling gas K for further cooling. The cooling gas K can be any one or a mixture of several of nitrogen, hydrogen, carbon monoxide, and methane. After cooling, the temperature of the metallized pellets G is less than 900℃.
[0065] In step S4, the metallized pellets G cooled by the cooling shaft furnace 64 are discharged into the annular cooler 7. After further cooling through cooling stages 71, 72, and 73, metallized pellets G that meet the requirements are obtained. These metallized pellets G can be used as low-carbon feedstock in blast furnace production. The metallized pellets G that meet the requirements have a metallization rate greater than 65%, a compressive strength greater than 2000 N / pellet, a drop strength of greater than 10 times from 2m, a drum strength greater than 90%, and an abrasion resistance index less than 5%. The metallized pellets G in cooling stage 71 are cooled to below 700°C, those in cooling stage 72 are cooled to below 400°C, and those in cooling stage 73 are cooled to below 100°C. The annular cooler 7 uses exhaust gas O with an oxygen content of less than 1%.
[0066] Furthermore, considering the rational recovery and utilization of heat, the flue gas generated by the rotary kiln 6 is transported to the preheating stage 54 via a flue gas pipeline. The flue gas from the preheating stage 54 is then transported to the drying stage 52 via a regenerating blower 55. The exhaust gas generated by the cooling stage 71 of the annular cooler 7 can be transported to the preheating stage 53 via a preheating blower 58 to preheat the carbon-containing pellets. The exhaust gas generated by the cooling stage 72 can be transported to the drying stage 51 via a drying blower 56 to dry the carbon-containing pellets.
[0067] In the preparation of metallized pellets G, the heat source for calcining the carbon-containing pellets mainly comes from the combustion of rotary kiln fuel H and primary combustion air I in the burner 63 at the kiln head. Simultaneously, secondary combustion air J is added near the kiln tail of the rotary kiln 6. This secondary combustion air J is injected through a combustion nozzle to ignite the reducing gas generated during the reduction of the carbon-containing pellets, providing heat for calcining the pellets. The high-temperature flue gas generated at the kiln tail of the rotary kiln 6 is introduced into the preheating stage 54 of the chain grate 7 to preheat the carbon-containing pellets. The high-temperature gas from the preheating stage 54 is then transported to the drying stage 52 via a regenerating fan 55 to dry the carbon-containing pellets.
[0068] The high-temperature exhaust gas generated in the first cooling stage 71 of the annular cooler 7 is transported to the first preheating stage 53 via the preheating fan 58 to preheat the carbon-containing pellets. The exhaust gas generated in the first preheating stage 53 and the second drying stage 52 is purified by the main exhaust fan 57 to generate purified exhaust gas III for discharge. The high-temperature exhaust gas generated in the second cooling stage 72 is transported to the first drying stage 51 via the drying fan 56 to dry the carbon-containing pellets. The exhaust gas generated in the first drying stage 51 is purified to generate purified exhaust gas II for discharge. The exhaust gas generated in the third cooling stage 73 is purified to generate purified exhaust gas I for discharge. The gas required for cooling by the annular cooler 7 (exhaust gas O) can be transported to the first cooling stage 71, the second cooling stage 72, and the third cooling stage 73 via the first cooling fan 74, the second cooling stage fan 75, and the third cooling stage fan 76 to force-cool the carbon-containing pellets.
[0069] In addition, this application also discloses an apparatus for producing metallized pellets, the apparatus comprising: a silo 1, a pelletizing machine 4, a chain grate machine 5, a rotary kiln 6, and an annular cooler 7.
[0070] The material silo 1 can preferably be multiple, for example, four. One material silo 1 is used to hold reducing coal A, the second material silo 1 is used to hold binder C, and the other two material silos 1 are used to hold iron ore powder B. After the iron ore powder B, reducing coal A, and binder C are fed into the material silo 1, the mixture D of the above three is transported to the mixer 3 via the conveyor belt 2 for mixing to form a homogenized material E. The briquetting machine 4 is connected to the mixer 3 and is used to pressure-form the homogenized material E to obtain carbon-containing green pellets F. The chain grate machine 5 is connected to the briquetting machine 4 and is used to dry and preheat the carbon-containing green pellets F on the chain grate machine 5. The chain grate machine 5 includes a drying section and a preheating section connected in sequence. The chain grate machine 5 is preferably composed of a drying section 51, a drying section 52, a preheating section 53, and a preheating section 54 connected in sequence. Rotary kiln 6 is connected to the preheating section 54 of chain grate 5. Rotary kiln 6 includes a high-temperature roasting section 61 and a cooling section 62, and cooling section 62 is connected to cooling shaft furnace 64. Rotary kiln 6 is connected to preheating section 54 via flue gas duct, and preheating section 54 is connected to drying section 52 via regenerating blower 55. Circular cooler 7 is connected to cooling shaft furnace 64. Circular cooler 7 includes multiple cooling sections connected in sequence at different cooling temperatures. Preferably, the circular cooler consists of a first cooling section 71, a second cooling section 72, and a third cooling section 73 connected in sequence at different cooling temperatures. The first cooling section 71 of circular cooler 7 is connected to preheating section 53 via preheating blower 58, and the second cooling section 72 of circular cooler 7 is connected to drying section 51 via drying blower 56.
[0071] The method and apparatus for producing metallized pellets in this application are simple in equipment, easy to operate, and have a wide range of applications. Compared with the traditional direct reduction technology of coal-based rotary kiln, they overcome the disadvantages of low production efficiency, complex process and narrow range of application.
[0072] The method for producing metallized pellets will be further explained below with reference to specific embodiments.
[0073] Example 1: As Figure 1 and Figure 2 As shown, in the method for producing metallized pellets G, iron ore powder B is hematite powder, reducing coal A is anthracite, and binder C is a composite binder prepared from bentonite and asphalt. The particle size of all raw materials is less than 0.09 mm. The mass ratios of hematite, anthracite, and binder in the mixture are 75%, 25%, and 5%, respectively. The moisture content of the mixture after adding water is 9%. The forming pressure of the briquetting machine 4 is 30 MPa. The drop strength (0.5 m) of the carbon-containing green pellets F is 6 times.
[0074] Carbon-containing green pellets F are fed into a chain grate machine 5, where they undergo drying and preheating. The flue gas temperature in the first drying stage 51 is 180℃ with an oxygen content of 8.5%; the flue gas temperature in the second drying stage 52 is 280℃ with an oxygen content of 5.8%; the flue gas temperature in the first preheating stage 53 is 360℃ with an oxygen content of 3.5%; and the flue gas temperature in the second preheating stage 54 is 630℃ with an oxygen content of 1.3%. The total drying and preheating time for the carbon-containing pellets in the chain grate machine 5 is 25 minutes. After preheating in the chain grate machine 5, the temperature of the carbon-containing pellets is 550℃, and their 0.5m drop strength is 18 times. The preheated carbon-containing pellets are then added to a rotary kiln 6 for calcination and reduction. The calcination and reduction temperature in the rotary kiln 6 is 1200℃, and the calcination and reduction time is 110 minutes.
[0075] After roasting, the metallized pellets are cooled in a cooling shaft furnace 64 using nitrogen gas. The cooled pellets reach a temperature of 850°C and are then discharged into an annular cooler 7 via a discharge device (not shown in the figure) for further cooling. The cooling gas used is waste gas O from a hot blast stove (not shown in the figure), with an oxygen content of 0.3%. Metallized pellets G in the first cooling stage 71 are cooled to 630°C by waste gas O. Metallized pellets G in the second cooling stage 72 are cooled to below 350°C by waste gas O. Finally, metallized pellets G in the third cooling stage 73 are cooled to 80°C by waste gas O before being discharged from the annular cooler 7, resulting in metallized pellets G that meet the requirements. Metallurgical performance analysis of the metallized pellets G reveals a metallization rate of 77%, a compressive strength of 2300 N / pellet, a 2m drop strength of 26 cycles, a drum strength of 96%, and an abrasion resistance index of 1.5%. These pellets can be used as auxiliary feedstock in blast furnaces for low-carbon ironmaking.
[0076] Examples 2-5: Compared with Example 1, Examples 2-5 differ in that the types of iron ore powder B and reducing coal A in step S1 are changed. The types of iron ore powder B and reducing coal A corresponding to Examples 2-5 are shown in Table 1:
[0077] Table 1. Types of iron ore powder B and reducing coal A corresponding to Examples 2-5.
[0078]
[0079]
[0080] The metallized pellets G obtained in Examples 2-5 that meet the requirements were subjected to metallurgical performance tests, and the results are shown in Table 2:
[0081] Table 2 shows the properties of the metallized pellets (hydrothermal carbon) prepared in Examples 2-5.
[0082]
[0083] As can be seen from Table 2, the metallization rate of the metallized pellets G prepared in Examples 2-5 is between 66% and 81%, the compressive strength is between 2030 and 2500 N, the 2m drop strength is between 18 and 32 cycles, the drum strength is between 92.1% and 97.3%, and the abrasion resistance index is between 1.3% and 4.3%. The metallized pellets G obtained can be used as auxiliary furnace charge for low-carbon ironmaking.
[0084] As can be seen from Examples 1 and 2, under the condition that anthracite is used for reducing coal A, the metallization rate of the metallized pellets G prepared from magnetite is lower than that prepared from hematite. This is mainly because hematite has higher reducibility than magnetite. Under the same roasting and reduction temperature and time, magnetite is reduced by reducing coal A to produce less metallic iron, resulting in a lower metallization rate. The compressive strength, drop strength, and drum strength of the metallized pellets G are mainly formed by the bonding and consolidation of metallic iron in the pellets under high-temperature conditions. Due to the low metallic iron content in the metallized pellets G prepared from magnetite, the compressive strength, drop strength, and drum strength of the pellets are lower. The abrasion resistance index decreases with increasing strength of the metallized pellets G, which can reduce the amount of powder generated during use and improve the blast furnace smelting effect.
[0085] As shown in Examples 1 and 4, when the iron ore powder B is all hematite, the metallization rate of the metallized pellets G prepared from semi-coke powder is greater than that prepared from anthracite. This is mainly because semi-coke powder is more reactive than anthracite. Under otherwise identical conditions, using semi-coke powder as a reducing agent accelerates the reduction of iron ore powder B, resulting in a higher metallization rate. Similarly, because the metallized pellets G prepared from semi-coke powder have a higher metallization rate, they exhibit better compressive strength, drop strength, and drum strength, and a lower abrasion index. This reduces the amount of powder generated during the use of the metallized pellets G, thus improving the blast furnace smelting effect.
[0086] Examples 6-11: Compared with Example 2, Examples 6-11 differ in that the calcination reduction temperature, calcination reduction time, and type of cooling gas K in step S3 are changed. The specific values of calcination reduction temperature, calcination reduction time, and type of cooling gas for each example are shown in Table 3.
[0087] Table 3 shows the calcination and reduction temperatures, calcination and reduction times, and types of cooling gases corresponding to Examples 6-11.
[0088]
[0089] The metallized pellets G prepared in Examples 6-11 were tested, and the results are shown in Table 4:
[0090] Table 4 shows the properties of the metallized pellets (hydrothermal carbon) prepared in Examples 6-11.
[0091]
[0092]
[0093] As can be seen from Table 4, the metallization rate of the metallized pellets G prepared in Examples 6-11 is between 69% and 81%, the compressive strength is between 2050 and 2290 N, the 2m drop strength is between 17 and 26 cycles, the drum strength is between 91.7% and 97.5%, and the abrasion resistance index is between 1.2% and 4.3%.
[0094] Therefore, increasing the calcination reduction temperature can accelerate the reduction rate of carbon-containing pellets, increase the metallization rate of metallized pellet G, and thus result in higher compressive strength, drop strength, and drum strength, while also exhibiting a lower abrasion index. Under the same calcination temperature conditions, extending the calcination reduction time can also improve the reduction effect of carbon-containing pellets, increase the metallization rate of metallized pellet G, and thus result in better compressive strength, drop strength, and drum strength, while also exhibiting a lower abrasion index.
[0095] When hydrogen and methane are used as cooling gases to cool high-temperature metallized pellets G, the iron oxides in the high-temperature metallized pellets G can be further reduced, thereby further improving the metallization rate of the metallized pellets G. Furthermore, methane, as a coolant, has a better reduction effect on the high-temperature metallized pellets G, resulting in metallized pellets G with good compressive strength, drop strength, and drum strength, as well as a low abrasion index. The above examples demonstrate that by increasing the roasting reduction temperature, extending the roasting reduction time, and using cooling gases with reducing properties, the metallurgical properties of the prepared high-strength metallized pellets G can be improved, making them suitable as auxiliary furnace charge for low-carbon ironmaking.
[0096] It should be noted that the hopper 1 and conveyor belt 2 provided in this embodiment can be any suitable existing structure. To clearly and concisely illustrate the technical solution provided in this embodiment, the above-mentioned parts will not be repeated here, and the accompanying drawings have also been simplified accordingly. However, it should be understood that this embodiment is not limited in scope as a result.
[0097] Multiple elements, components, parts, or steps can be provided by a single integrated element, component, part, or step. Alternatively, a single integrated element, component, part, or step can be divided into multiple separate elements, components, parts, or steps. The use of "a" or "an" to describe an element, component, part, or step does not imply the exclusion of other elements, components, parts, or steps.
[0098] It should be understood that the above description is for illustrative purposes and not for limitation. Many embodiments and applications beyond the provided examples will be apparent to those skilled in the art upon reading the above description. Therefore, the scope of this teaching should not be determined by reference to the above description, but rather by reference to the foregoing claims and the full scope of their equivalents. For purposes of completeness, all articles and references, including patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the foregoing claims is not intended as a waiver of that subject matter, nor should it be construed as an indication that the applicant has not considered that subject matter as part of the disclosed application subject matter.
Claims
1. A method for producing metallized pellets, characterized in that, Includes the following steps: S1. Iron ore powder, reducing coal, binder, and water are mixed in a predetermined mass ratio, and the mixture is pressure-molded to obtain carbon-containing green pellets; wherein, the predetermined mass ratio is 65%-80% iron ore powder, 8%-16% reducing coal, 2%-10% binder, and 5%-15% moisture. S2. The carbon-containing pellets are dried and preheated on a chain grate machine to obtain preheated carbon-containing pellets. The chain grate machine includes a drying section, a drying section, a preheating section, and a preheating section connected in sequence. The flue gas temperature of the drying section is less than 200°C and the oxygen content is less than 10%. The flue gas temperature of the drying section is less than 300°C and the oxygen content is less than 7%. The flue gas temperature of the preheating section is less than 400°C and the oxygen content is less than 4%. The flue gas temperature of the preheating section is less than 700°C and the oxygen content is less than 2%. The total drying and preheating time of the carbon-containing pellets on the chain grate machine is 20-60 minutes. S3. The preheated carbon-containing pellets are calcined in a rotary kiln to prepare metallized pellets by self-reduction. The rotary kiln includes a high-temperature calcination section and a cooling section, which are connected. The flue gas generated by the rotary kiln is transported to the preheating stage through a flue gas pipeline, and the flue gas from the preheating stage is transported to the drying stage through a regenerating fan. The rotary kiln head is equipped with a burner to provide roasting heat through the combustion of fuel and primary combustion air. At the same time, a combustion-supporting spray gun is set in the area near the kiln tail of the rotary kiln to inject secondary combustion air into the rotary kiln. The combustion-supporting spray gun ignites the reducing gas generated by the carbon-containing pellets during the self-reduction process of roasting in the rotary kiln. The heat generated by the combustion of the reducing gas is used to assist in the roasting of the carbon-containing pellets. S4. The metallized pellets are cooled in an annular cooler to obtain metallized pellet products. The annular cooler includes multiple cooling sections connected in sequence with different cooling temperatures. The multiple cooling sections connected in sequence include a first cooling section, a second cooling section, and a third cooling section connected in sequence. The exhaust gas generated by the first cooling section is transported to the first preheating section by a preheating fan, and the exhaust gas generated by the second cooling section is transported to the first drying section by a drying blower.
2. The method for producing metallized pellets according to claim 1, characterized in that, The iron ore powder is any one or a mixture of several of hematite, magnetite, limonite, and vanadium-titanium magnetite.
3. The method for producing metallized pellets according to claim 1, characterized in that, The reduced coal includes any one or a mixture of several of anthracite, lean coal, semi-coke powder, and coke powder.
4. The method for producing metallized pellets according to claim 1, characterized in that, The adhesive is any one or a mixture of two of the following: organic adhesive and inorganic adhesive.
5. The method for producing metallized pellets according to claim 1, characterized in that, The iron ore powder, reducing coal, and binder have a particle size of less than 0.1 mm.
6. The method for producing metallized pellets according to claim 1, characterized in that, In step S1, the molding pressure for pressure molding of the mixed material is 10MPa-50MPa, and the carbon-containing pellets have a drop strength of more than 5 times at 0.5m.
7. The method for producing metallized pellets according to claim 1, characterized in that, In step S2, the temperature of the preheated carbon-containing pellets is greater than 300°C, and the 0.5m drop strength of the preheated carbon-containing pellets is greater than 10 times.
8. The method for producing metallized pellets according to claim 1, characterized in that, In step S3, the calcination and reduction temperature of the rotary kiln is 1150℃-1300℃, and the calcination and reduction time is 30-180min.
9. The method for producing metallized pellets according to claim 1, characterized in that, In step S3, the metallized pellets calcined in the rotary kiln need to be cooled in a cooling shaft furnace. The cooling gas is any one or a mixture of several of nitrogen, hydrogen, carbon monoxide, and methane. After cooling, the temperature of the metallized pellets is less than 900°C.
10. The method for producing metallized pellets according to claim 1, characterized in that, The metallized pellets in the first cooling stage are cooled to a temperature below 700°C, the metallized pellets in the second cooling stage are cooled to a temperature below 400°C, and the metallized pellets in the third cooling stage are cooled to a temperature below 100°C.
11. The method for producing metallized pellets according to claim 1, characterized in that, The ring cooler uses gas cooling, and the gas is exhaust gas with an oxygen content of less than 1%.
12. The method for producing metallized pellets according to claim 1, characterized in that, In step S4, the metallization rate of the cooled metallized pellets is greater than 65%, the compressive strength is greater than 2000N / pellet, the drop strength at 2m is greater than 10 times, the drum strength is greater than 90%, and the wear resistance index is less than 5%.
13. An apparatus for producing metallized pellets, characterized in that, include: The silos are used to hold iron ore powder, reducing coal, and binder respectively. The mixing machine is used to mix the iron ore powder, reducing coal, and binder after they are fed from the hopper to form a homogenized mixture. A briquetting machine, connected to the mixer, is used to press the mixed material into carbon-containing green briquettes. A chain grate machine, connected to the briquetting machine, is used to dry and preheat the carbon-containing raw pellets on the chain grate machine. The chain grate machine includes a drying section, a drying section, a preheating section, and a preheating section connected in sequence. A rotary kiln is connected to the preheating section of the chain grate machine. The rotary kiln includes a high-temperature roasting section and a cooling section. A burner is provided at the kiln head of the rotary kiln, and a combustion-supporting spray gun is provided near the kiln tail. The combustion-supporting spray gun is used to inject secondary combustion-supporting air to ignite the reducing gas generated during the self-reduction process of the carbon-containing pellets in the rotary kiln, and to use the heat generated by the combustion of the reducing gas to assist in roasting. The rotary kiln is connected to the second preheating section via a flue gas duct, and the second preheating section is connected to the second drying section via a regenerative fan. A cooling vertical furnace, wherein the cooling section is connected to the cooling vertical furnace; An annular cooler is connected to the cooling vertical furnace. The annular cooler includes multiple cooling sections connected in sequence with different cooling temperatures. The multiple cooling sections connected in sequence include a first cooling section, a second cooling section, and a third cooling section connected in sequence. The first cooling section is connected to the first preheating section via a preheating fan, and the second cooling section is connected to the first drying section via a drying fan.
Citation Information
Patent Citations
Method for producing metallized iron-smelting raw material
CN101070562A
Chain grate-tandem type rotary kiln direct reduction technology for refractory low-grade micro-fine iron ore
CN104164527A