A mildew-resistant nylon material and its preparation method

By using maleic anhydride-grafted elastomer as a carrier, the organic antifungal agent was mastered and mixed with nylon material, which solved the problem of performance degradation of organic antifungal agents at high temperatures, and achieved high-efficiency antibacterial and antifungal effect and cost reduction of glass fiber reinforced nylon material.

CN116656072BActive Publication Date: 2026-11-10NANJING JULONG SCIENCE & TECHNOLOGY CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310652929.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2026-11-10
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

Existing organic antifungal agents have poor high-temperature resistance and cannot be effectively applied to nylon materials, especially glass fiber reinforced nylon materials, resulting in poor antibacterial and antifungal effects.

Method used

Maleic anhydride-grafted elastomer is used as a carrier for the organic antifungal agent. The organic antifungal agent is masterbatched and mixed with nylon material to avoid the impact of high temperature and strong shear on its performance and improve the antibacterial and antifungal effect.

Benefits of technology

It effectively improves the antibacterial and antifungal effect of organic antifungal agents in nylon materials, especially glass fiber reinforced nylon materials, reduces the amount added and lowers production costs, and is simple to operate and easy to apply industrially.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses an anti-mildew nylon material, comprising the following components in parts by weight: 2-3 parts of organic anti-mildew agent masterbatch, and 96-99 parts of glass fiber reinforced nylon material. The organic anti-mildew agent comprises the following components in parts by weight: 75-85 parts of maleic anhydride-grafted elastomer, 15-25 parts of organic anti-mildew agent, 0.2-0.5 parts of antioxidant, and 0.3-0.5 parts of lubricant. In the preparation process, by using maleic anhydride-grafted elastomer as a carrier for the organic anti-mildew agent, and granulating the organic anti-mildew agent before mixing it with the nylon material, the antibacterial and anti-mildew properties of the organic anti-mildew agent are effectively avoided from being affected by the high temperature and strong shearing action in the twin-screw extruder during nylon material granulation. This improves the antibacterial and anti-mildew effect of the organic anti-mildew agent when applied to nylon materials, especially glass fiber reinforced nylon materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of engineering plastics technology, specifically relating to an anti-mildew nylon material and its preparation method. Background Technology

[0002] Nylon, also known as polyamide, is a general term for thermoplastic resins containing repeating amide groups -[NHCO]- in its main chain. It is a high-performance engineering plastic. However, as a nitrogen-containing polymer, nylon can provide a nitrogen source for microbial growth. Combined with its hygroscopic nature, its products are prone to mold growth, severely impacting their use and maintenance. Currently, antibacterial and antifungal agents are typically added during the melting process to improve the antifungal effect of nylon materials. Existing antifungal agents commonly used in the technology mainly include inorganic antibacterial and antifungal agents (such as silver ion antibacterial agents) and organic antifungal agents. Inorganic antibacterial and antifungal agents have low antibacterial and antifungal effects, requiring a higher proportion for mold inhibition, leading to higher production costs. Furthermore, silver ions can cause discoloration and affect material properties during processing. Compared to inorganic antibacterial and antifungal agents, organic antifungal agents offer better antifungal effects and exhibit better compatibility with polymers, resulting in lower dosages. Furthermore, organic antifungal agents do not affect the color or physical properties of materials, making their application in polymers more widespread. However, in practical applications, it has been found that the performance of organic antifungal agents deteriorates significantly with processing temperatures exceeding 200°C. Nylon materials require high-temperature extrusion granulation during manufacturing, especially glass fiber reinforced nylon, where the extrusion granulation temperature requirements are even higher. Therefore, conventionally used organic antifungal agents in existing technologies do not achieve satisfactory antibacterial and antifungal effects when applied to nylon materials, particularly glass fiber reinforced nylon. Summary of the Invention

[0003] To address the technical problem that existing organic antifungal agents have poor high-temperature resistance and cannot be applied to nylon materials, especially glass fiber reinforced nylon materials, this invention proposes an antifungal nylon material and its preparation method. By using maleic anhydride-grafted elastomer as a carrier for the organic antifungal agent, the organic antifungal agent is masterbatched and then mixed with the nylon material. This effectively avoids the impact of high temperature and strong shearing in the twin-screw extruder on the antibacterial and antifungal properties of the organic antifungal agent during nylon material granulation, thereby improving the antibacterial and antifungal effect of the organic antifungal agent when applied to nylon materials, especially glass fiber reinforced nylon materials.

[0004] To achieve the above objectives, the present invention adopts the following technical solution:

[0005] An organic antifungal agent masterbatch comprises the following components in parts by weight:

[0006]

[0007] Furthermore, the maleic anhydride grafted elastomer is a maleic anhydride grafted elastomer with a melting point below 150°C.

[0008] Furthermore, the maleic anhydride-grafted elastomer is any one of maleic anhydride-grafted POE, maleic anhydride-grafted EPDM, or maleic anhydride-grafted PE.

[0009] Furthermore, the organic antifungal agent is one or a mixture of any two or more of the following: quaternary ammonium salts, biguanides, benzoates, pyridines, imidazoles, and haloamines, in any proportion.

[0010] Furthermore, the antioxidant is a compound formed by mixing antioxidant 1098 and antioxidant 168 in a weight ratio of (0.5-1):1.

[0011] Furthermore, the lubricant is one or a mixture of any two or more of calcium stearate, zinc stearate, ethylene bis-stearamide, polyethylene wax, and polydimethylsiloxane in any proportion.

[0012] A mildew-resistant nylon material, comprising the following components in parts by weight:

[0013] 2-3 parts of organic antifungal masterbatch

[0014] 96-99 parts of glass fiber reinforced nylon material

[0015] The organic antifungal agent masterbatch is any one of the above-mentioned organic antifungal agent masterbatches.

[0016] Furthermore, the glass fiber reinforced nylon material is any one of glass fiber reinforced PA66, glass fiber reinforced PA6, or glass fiber reinforced PA66 / PA6 alloy.

[0017] A method for preparing an anti-mildew nylon material includes the following steps:

[0018] Preparation of organic antifungal agent masterbatch

[0019] Weigh out the maleic anhydride-grafted elastomer, organic mildew inhibitor, antioxidant and lubricant according to the weight parts, mix the weighed components evenly, and then melt-extrude and granulate to obtain organic mildew inhibitor masterbatch.

[0020] Preparation of anti-mildew nylon materials

[0021] Weigh the organic anti-mildew agent masterbatch and glass fiber reinforced nylon material according to the weight parts, and put the weighed components into the mixer in sequence and mix them evenly to obtain the anti-mildew nylon material.

[0022] Furthermore, the temperature of the melt extrusion granulation is 160–200°C.

[0023] The beneficial effects of this invention are:

[0024] This invention utilizes maleic anhydride-grafted elastomers as carriers for organic antifungal agents. The organic antifungal agents are mastered and then mixed with nylon materials. This effectively avoids the impact of high temperatures and strong shearing in the twin-screw extruder on the antibacterial and antifungal properties of the organic antifungal agents during nylon material granulation, thereby improving the antibacterial and antifungal effect of the organic antifungal agents when applied to nylon materials, especially glass fiber reinforced nylon materials.

[0025] This invention maximizes the antibacterial and antifungal effects of organic antifungal agents by using maleic anhydride-grafted elastomers as carriers and mixing the organic antifungal agents with nylon materials after mastering the organic antifungal agents. This effectively reduces the amount of organic antifungal agents added, thereby reducing the production cost of nylon materials and facilitating their industrial application.

[0026] The organic anti-mildew masterbatch of the present invention is produced by melt extrusion granulation, and the anti-mildew nylon material is obtained by mixing the organic anti-mildew masterbatch and glass fiber reinforced nylon material through a mixer. The entire preparation process does not require special or precision equipment and instruments, and the preparation process is simple and easy to operate, which is conducive to industrial promotion and application. Detailed Implementation

[0027] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the described embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art to which this invention pertains.

[0028] The terms "first," "second," and similar words used in the specification and claims of this patent application do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Similarly, unless the context clearly indicates otherwise, the singular forms of "an," "a," or "the," etc., do not indicate a quantity limitation, but rather indicate the presence of at least one. Terms such as "comprising" or "including" indicate that the element or object preceding "comprising" encompasses the features, integrals, steps, operations, elements, and / or components listed following "comprising" or "including," and do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components, and / or collections thereof. Terms such as "upper," "lower," "left," and "right" are used only to indicate relative positional relationships; these relative positional relationships may change accordingly when the absolute position of the described object changes.

[0029] Example 1

[0030] A method for preparing an anti-mildew nylon material includes the following steps:

[0031] Preparation of organic antifungal agent masterbatch

[0032] Weigh each component according to the following parts by weight:

[0033] 75 parts of maleic anhydride-grafted elastomer, 24.3 parts of organic antifungal agent, 0.2 parts of antioxidant, and 0.5 parts of lubricant were weighed and mixed evenly. The mixture was then melt-extruded and granulated at 190°C to obtain organic antifungal agent masterbatch.

[0034] The maleic anhydride-grafted elastomer is maleic anhydride-grafted POE, the organic antifungal agent is polyhexyl biguanide, the antioxidant is a compound of antioxidant 1098 and antioxidant 168 mixed in a weight ratio of 1:1, and the lubricant is ethylene bis-stearamide.

[0035] Preparation of anti-mildew nylon materials

[0036] Weigh each component according to the following parts by weight:

[0037] Two parts of organic anti-mildew agent masterbatch and 98 parts of glass fiber reinforced nylon material are weighed and placed into a medium-speed mixer and mixed evenly to obtain anti-mildew nylon material.

[0038] Among them, the glass fiber reinforced nylon material is glass fiber reinforced PA66-GF30 material.

[0039] The preparation method of the glass fiber reinforced PA66-GF30 material is as follows:

[0040] Weigh each component according to the following parts by weight:

[0041] 69.3 parts PA66, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0042] PA66, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the glass fiber reinforced PA66-GF30 material was obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 265℃, Zone 2 260℃, Zone 3 260℃, Zone 4 255℃, Zone 5 250℃, Zone 6 245℃, Zone 7 240℃, Zone 8 235℃, Zone 9 230℃, Zone 10 230℃, and the die head temperature was 265℃.

[0043] Example 2

[0044] A method for preparing an anti-mildew nylon material includes the following steps:

[0045] Preparation of organic antifungal agent masterbatch

[0046] Weigh each component according to the following parts by weight:

[0047] 84 parts of maleic anhydride grafted elastomer, 15.2 parts of organic mildew inhibitor, 0.5 parts of antioxidant, and 0.3 parts of lubricant were weighed and mixed evenly. The mixture was then melt-extruded and granulated at 160°C to obtain organic mildew inhibitor masterbatch.

[0048] The maleic anhydride-grafted elastomer is maleic anhydride-grafted EPDM, the organic antifungal agent is an organosilicon quaternary ammonium salt, the antioxidant is a compound of antioxidant 1098 and antioxidant 168 mixed in a weight ratio of 1:1, and the lubricant is ethylene bis-stearamide.

[0049] Preparation of anti-mildew nylon materials

[0050] Weigh each component according to the following parts by weight:

[0051] Three parts of organic anti-mildew agent masterbatch and 97 parts of glass fiber reinforced nylon material are weighed and placed into a medium-speed mixer and mixed evenly to obtain anti-mildew nylon material.

[0052] Among them, the glass fiber reinforced nylon material is glass fiber reinforced PA6-GF30 material.

[0053] The preparation method of the glass fiber reinforced PA6-GF30 material is as follows:

[0054] Weigh each component according to the following parts by weight:

[0055] 69.3 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0056] PA6, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the glass fiber reinforced PA66-GF30 material was obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 255℃, Zone 2 250℃, Zone 3 250℃, Zone 4 245℃, Zone 5 245℃, Zone 6 240℃, Zone 7 235℃, Zone 8 230℃, Zone 9 220℃, Zone 10 220℃, and the die head temperature was 250℃.

[0057] Example 3

[0058] A method for preparing an anti-mildew nylon material includes the following steps:

[0059] Preparation of organic antifungal agent masterbatch

[0060] Weigh each component according to the following parts by weight:

[0061] 80 parts of maleic anhydride grafted elastomer, 19.3 parts of organic mildew inhibitor, 0.3 parts of antioxidant, and 0.4 parts of lubricant were weighed and mixed evenly. The mixture was then melt-extruded and granulated at 170°C to obtain organic mildew inhibitor masterbatch.

[0062] The maleic anhydride-grafted elastomer is maleic anhydride-grafted PE, the organic antifungal agent is 2-pyridinephenol-1-oxide sodium, the antioxidant is a compound of antioxidant 1098 and antioxidant 168 mixed in a weight ratio of 0.5:1, and the lubricant is ethylene bis-stearamide.

[0063] Preparation of anti-mildew nylon materials

[0064] Weigh each component according to the following parts by weight:

[0065] 2.5 parts of organic anti-mildew agent masterbatch and 97.5 parts of glass fiber reinforced nylon material are weighed and placed into a medium-speed mixer and mixed evenly to obtain anti-mildew nylon material.

[0066] Among them, the glass fiber reinforced nylon material is glass fiber reinforced PA66 / PA6-GF30 material.

[0067] The preparation method of the glass fiber reinforced PA66 / PA6-GF30 material is as follows:

[0068] Weigh each component according to the following parts by weight:

[0069] 50 parts PA66, 19.3 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0070] PA66, PA6, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the glass fiber reinforced PA66-GF30 material was obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 265℃, Zone 2 260℃, Zone 3 260℃, Zone 4 255℃, Zone 5 250℃, Zone 6 245℃, Zone 7 240℃, Zone 8 235℃, Zone 9 230℃, Zone 10 230℃, and the die head temperature was 265℃.

[0071] Example 4

[0072] A method for preparing an anti-mildew nylon material includes the following steps:

[0073] Preparation of organic antifungal agent masterbatch

[0074] Weigh each component according to the following parts by weight:

[0075] 75 parts of maleic anhydride-grafted elastomer, 24.3 parts of organic antifungal agent, 0.2 parts of antioxidant, and 0.5 parts of lubricant were weighed and mixed evenly. The mixture was then melt-extruded and granulated at 180°C to obtain organic antifungal agent masterbatch.

[0076] The maleic anhydride-grafted elastomer is maleic anhydride-grafted POE, the organic antifungal agent is 2-(4-thiazolyl)benzimidazole, the antioxidant is a compound of antioxidant 1098 and antioxidant 168 mixed in a weight ratio of 1:1, and the lubricant is ethylene bis-stearamide.

[0077] Preparation of anti-mildew nylon materials

[0078] Weigh each component according to the following parts by weight:

[0079] Two parts of organic anti-mildew agent masterbatch and 98 parts of glass fiber reinforced nylon material are weighed and placed into a medium-speed mixer and mixed evenly to obtain anti-mildew nylon material.

[0080] Among them, the glass fiber reinforced nylon material is glass fiber reinforced PA66-GF30 material.

[0081] The preparation method of the glass fiber reinforced PA66-GF30 material is as follows:

[0082] Weigh each component according to the following parts by weight:

[0083] 69.3 parts PA66, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0084] PA66, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the glass fiber reinforced PA66-GF30 material was obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 265℃, Zone 2 260℃, Zone 3 260℃, Zone 4 255℃, Zone 5 250℃, Zone 6 245℃, Zone 7 240℃, Zone 8 235℃, Zone 9 230℃, Zone 10 230℃, and the die head temperature was 265℃.

[0085] Example 5

[0086] A method for preparing an anti-mildew nylon material includes the following steps:

[0087] Preparation of organic antifungal agent masterbatch

[0088] Weigh each component according to the following parts by weight:

[0089] 75 parts of maleic anhydride-grafted elastomer, 24.3 parts of organic antifungal agent, 0.2 parts of antioxidant, and 0.5 parts of lubricant were weighed and mixed evenly. The mixture was then melt-extruded and granulated at 180°C to obtain organic antifungal agent masterbatch.

[0090] The maleic anhydride-grafted elastomer is maleic anhydride-grafted POE, the organic antifungal agent is a halogenated amine organic antifungal agent, the antioxidant is a compound composed of antioxidant 1098 and antioxidant 168 mixed in a weight ratio of 1:1, and the lubricant is ethylene bis-stearamide.

[0091] Preparation of anti-mildew nylon materials

[0092] Weigh each component according to the following parts by weight:

[0093] Two parts of organic anti-mildew agent masterbatch and 98 parts of glass fiber reinforced nylon material are weighed and placed into a medium-speed mixer and mixed evenly to obtain anti-mildew nylon material.

[0094] Among them, the glass fiber reinforced nylon material is glass fiber reinforced PA66-GF30 material.

[0095] The preparation method of the glass fiber reinforced PA66-GF30 material is as follows:

[0096] Weigh each component according to the following parts by weight:

[0097] 69.3 parts PA66, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0098] PA66, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the glass fiber reinforced PA66-GF30 material was obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 265℃, Zone 2 260℃, Zone 3 260℃, Zone 4 255℃, Zone 5 250℃, Zone 6 245℃, Zone 7 240℃, Zone 8 235℃, Zone 9 230℃, Zone 10 230℃, and the die head temperature was 265℃.

[0099] Comparative Example 1

[0100] A method for preparing a nylon material includes the following steps:

[0101] Weigh each component according to the following parts by weight:

[0102] 69.3 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 30 parts chopped glass fiber;

[0103] PA6, antioxidant 168, antioxidant 1098, and calcium stearate were weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers were side-fed, and the mixture was extruded through the twin-screw extruder to obtain glass fiber reinforced PA66 material. The temperatures of each zone of the twin-screw extruder were as follows: Zone 1 255℃, Zone 2 250℃, Zone 3 250℃, Zone 4 245℃, Zone 5 245℃, Zone 6 240℃, Zone 7 235℃, Zone 8 230℃, Zone 9 220℃, Zone 10 220℃, and the die head temperature was 250℃.

[0104] The difference between Comparative Example 1 and Example 2 above is that the nylon material is treated with anti-mildew agents.

[0105] Comparative Example 2

[0106] A method for preparing an anti-mildew nylon material includes the following steps:

[0107] Weigh each component according to the following parts by weight:

[0108] 68.8 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 0.5 parts organosilicon quaternary ammonium salt, 30 parts chopped glass fiber;

[0109] PA6, antioxidant 168, antioxidant 1098, calcium stearate, and organosilicon quaternary ammonium salt are weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers are side-fed, and glass fiber reinforced PA66 material is obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are as follows: Zone 1 255℃, Zone 2 250℃, Zone 3 250℃, Zone 4 245℃, Zone 5 245℃, Zone 6 240℃, Zone 7 235℃, Zone 8 230℃, Zone 9 220℃, Zone 10 220℃, and the die head temperature is 250℃.

[0110] The difference between Comparative Example 2 and Example 2 above is that the organic antifungal agent was not loaded onto the maleic anhydride-grafted elastomer, but was directly added to the nylon material for extrusion.

[0111] Comparative Example 3

[0112] A method for preparing an anti-mildew nylon material includes the following steps:

[0113] Weigh each component according to the following parts by weight:

[0114] 67.3 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 0.5 parts organosilicon quaternary ammonium salt, 1.5 parts maleic anhydride grafted PE, 30 parts chopped glass fiber;

[0115] PA6, antioxidant 168, antioxidant 1098, calcium stearate, organosilicon quaternary ammonium salt, and maleic anhydride-grafted PE are sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers are side-fed, and glass fiber reinforced PA66 material is obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are as follows: Zone 1 255℃, Zone 2 250℃, Zone 3 250℃, Zone 4 245℃, Zone 5 245℃, Zone 6 240℃, Zone 7 235℃, Zone 8 230℃, Zone 9 220℃, Zone 10 220℃, and the die head temperature is 250℃.

[0116] The difference between Comparative Example 3 and Example 2 is that the organic fungicide was not loaded onto the maleic anhydride-grafted PE; instead, the organic fungicide and maleic anhydride-grafted PE were directly added to the nylon material for extrusion. The difference between Comparative Example 3 and Comparative Example 2 is that maleic anhydride-grafted PE was not added in Comparative Example 2.

[0117] Comparative Example 4

[0118] A method for preparing an anti-mildew nylon material includes the following steps:

[0119] Weigh each component according to the following parts by weight:

[0120] 67.3 parts PA6, 0.15 parts antioxidant 168, 0.15 parts antioxidant 1098, 0.4 parts calcium stearate, 3 parts organosilicon quaternary ammonium salt, 30 parts chopped glass fiber;

[0121] PA6, antioxidant 168, antioxidant 1098, calcium stearate, and organosilicon quaternary ammonium salt are weighed and sequentially added to the barrel of a twin-screw extruder. Short-cut glass fibers are side-fed, and glass fiber reinforced PA66 material is obtained by extrusion through the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are as follows: Zone 1 255℃, Zone 2 250℃, Zone 3 250℃, Zone 4 245℃, Zone 5 245℃, Zone 6 240℃, Zone 7 235℃, Zone 8 230℃, Zone 9 220℃, Zone 10 220℃, and the die head temperature is 250℃.

[0122] The difference between Comparative Example 4 and Comparative Example 2 above is that the amount of organosilicon added is increased from 0.5 parts to 3 parts.

[0123] Performance testing

[0124] To verify the antibacterial and antifungal properties of the nylon materials obtained in the above embodiments and comparative examples, the nylon materials obtained in the above embodiments and comparative examples were injection molded into 60×60 samples, and antibacterial and antifungal tests were conducted according to two standards: IEC 60068-2-10 and GB / T31402-2015. The test results of each embodiment and comparative example are shown in Table 1 below:

[0125] Table 1. Antibacterial and antifungal test results of each example and comparative example.

[0126] Serial Number Anti-mildew rating Antibacterial rate (E. coli) Antibacterial rate (Staphylococcus aureus) Example 1 Level 0 99.9 (R value 3.8) 99.9 (R value 4.6) Example 2 Level 0 99.9 (R value 4.0) 99.9 (R value 5.4) Example 3 Level 0 99.9 (R value 3.5) 99.9 (R value 4.9) Example 4 Level 0 99.9 (R value 3.6) 99.9 (R value 4.7) Example 5 Level 0 99.9 (R value 3.9) 99.9 (R value 4.6) Comparative Example 1 Level 3 98.1 (R value 1.7) 99.5 (R value 2.3) Comparative Example 2 2a level 98.8 (R value 2.5) 99.7 (R value 2.9) Comparative Example 3 2a level 99.1 (R value 2.8) 99.7 (R value 3.0) Comparative Example 4 Level 1 99.6 (R value 3.2) 99.8 (R value 3.3)

[0127] As shown in the test results of Examples 1-5 in Table 1 above, the nylon material obtained by the preparation method of this invention has excellent antibacterial and antifungal effects. Combining the test results of Comparative Examples 1, 2, and 4, it can be seen that compared to nylon material without added antifungal agents, while adding organic antifungal agents directly during the nylon extrusion process can improve the antibacterial and antifungal effects of the nylon material to some extent, the overall effect is not ideal. Even after increasing the amount of organic antifungal agent to 3% as in Comparative Example 4, the antifungal grade of the nylon material only reaches level 1, and the antibacterial effect needs further improvement. Furthermore, the test results of Comparative Example 3 show that its antibacterial and antifungal effects are also not ideal. Therefore, directly extruding and mixing organic antifungal agents with nylon materials can severely affect the antibacterial and antifungal effects of the organic antifungal agents. This invention uses maleic anhydride-grafted elastomers as carriers for organic antifungal agents, and then mixes the organic antifungal agents with nylon materials after mastering them. This effectively avoids the situation where the high temperature and strong shearing action in the twin-screw extruder affects the antibacterial and antifungal performance of the organic antifungal agents during nylon material granulation, thereby improving the antibacterial and antifungal effect of the organic antifungal agents when applied to nylon materials, especially glass fiber reinforced nylon materials.

[0128] Finally, it should be noted that these embodiments are for illustrative purposes only and do not limit the scope of the invention. Furthermore, those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively list all embodiments here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A mildew-resistant nylon material, characterized in that, The components include the following parts by weight: 2-3 parts of organic antifungal masterbatch 96-99 parts of glass fiber reinforced nylon material The organic antifungal agent masterbatch is composed of the following components in parts by weight: 75-85 parts of maleic anhydride-grafted elastomer 15-25 parts of organic antifungal agent Antioxidant 0.2-0.5 parts 0.3-0.5 parts lubricant The maleic anhydride grafted elastomer is a maleic anhydride grafted elastomer with a melting point below 150°C. The preparation method of the organic antifungal agent masterbatch is as follows: weigh maleic anhydride grafted elastomer, organic antifungal agent, antioxidant and lubricant according to the weight parts, mix the weighed components evenly, and then melt extrude and granulate to obtain organic antifungal agent masterbatch. The temperature of the melt extrusion granulation is 160~200℃.

2. The anti-mildew nylon material according to claim 1, characterized in that: The maleic anhydride-grafted elastomer is either maleic anhydride-grafted POE or maleic anhydride-grafted EPDM.

3. The anti-mildew nylon material according to claim 1, characterized in that: The organic antifungal agent is one or a mixture of any two or more of the following: quaternary ammonium salts, biguanides, benzoates, pyridines, imidazoles, and haloamines, in any proportion.

4. The anti-mildew nylon material according to claim 1, characterized in that: The antioxidant is a compound formed by mixing antioxidant 1098 and antioxidant 168 in a weight ratio of (0.5~1):

1.

5. The anti-mildew nylon material according to claim 1, characterized in that: The lubricant is one or a mixture of any two or more of the following: calcium stearate, zinc stearate, ethylene bis-stearamide, polyethylene wax, and polydimethylsiloxane, in any proportion.

6. The anti-mildew nylon material according to claim 1, characterized in that: The glass fiber reinforced nylon material is any one of glass fiber reinforced PA66, glass fiber reinforced PA6, or glass fiber reinforced PA66 / PA6 alloy.

7. A method for preparing the anti-mildew nylon material as described in claim 1, characterized in that, Includes the following steps: Preparation of organic antifungal agent masterbatch Weigh out maleic anhydride-grafted elastomer, organic mildew inhibitor, antioxidant and lubricant, mix the weighed components evenly, and then melt-extrude and granulate to obtain organic mildew inhibitor masterbatch. Preparation of anti-mildew nylon materials Weigh out the organic anti-mildew agent masterbatch and glass fiber reinforced nylon material, and put the weighed components into a mixer in sequence and mix them evenly to obtain the anti-mildew nylon material.

Citation Information

Patent Citations

  • Antibacterial reinforced nylon material and preparation method thereof

    CN103788645A

  • Color master batch as well as preparation method and application thereof

    CN113999479A

  • Mildew-proof reinforced nylon 6 master batch and preparation method thereof

    CN114805865A