High entropy alloy layer and preparation method thereof

The deposit of high-entropy alloy layer by laser cladding technology solves the problems of slow cooling speed and component segregation in the prior art, and achieves the improvement of hardness and wear resistance of high-entropy alloy layer, which is suitable for the rapid manufacturing of complex structures.

CN116657018BInactive Publication Date: 2024-11-01UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310688433.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-12
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing high-entropy alloy preparation methods have slow cooling speed, which is prone to component segregation, and is not easy to form complex structural parts, which limits their use in practical applications.

Method used

Laser cladding technology is used to deposit high-entropy alloy layer. Through the deposition of five layers, each layer consists of at least two sublayers, and the hardness is gradually increased. From the inside to the outside, it is FeCrCoNi, FeCrCoNiMo0.5, and FeCrCoNiMo0.5W0. 25. FeCrCoNiMo0.5W0.5 and FeCrCoNiMo0.5W0.75 use laser additive systems to achieve high-precision and density metal parts forming.

Benefits of technology

The hardness and wear resistance of high-entropy alloy layer are improved, the material structure is more stable, adapted to heavy-duty environments, and has good wear resistance, and is suitable for rapid manufacturing of complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116657018B_ABST
    Figure CN116657018B_ABST
Patent Text Reader

Abstract

The present invention discloses a high entropy alloy layer component and a preparation method thereof. In an embodiment of the present invention, the prepared high entropy alloy layer component has multiple high entropy alloy layers, and the hardness increases from the inside to the outside. Based on the gradient change of the hardness, it can adapt to application environments such as heavy loads. And each high entropy alloy layer has at least two sublayers, which can make the corresponding high entropy alloy layer structure more stable and have a better transition effect as a whole. In addition, the wear resistance of the prepared high entropy alloy layer with five layers is also relatively good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high entropy alloy layer component prepared on the surface of a workpiece, and a method for preparing the high entropy alloy layer component, wherein the high entropy alloy layer component is a workpiece having a high entropy alloy layer on the surface. Background Art

[0002] High-entropy alloys (HEA) are alloys formed by five or more equal or approximately equal amounts of metals. Since high-entropy alloys may have many ideal properties, they are highly valued in materials science and engineering. In the past, alloys may have only one or two main metal components. For example, iron is used as the basis, and some trace elements are added to improve its properties, so the result is an iron-based alloy. In the past, if more metal types are added to the alloy, the material will become brittle. However, high-entropy alloys are different from previous alloys. There are multiple metals that will not become brittle, and they are a new material.

[0003] High entropy alloys were first proposed in the 1990s, but it was not until 2010 that many related studies were conducted and related products were gradually launched. In recent years, high entropy alloy products have experienced explosive growth.

[0004] The alloy exhibits a multi-principal high entropy effect, can form a simple solid solution structure, and has excellent comprehensive properties. At present, high entropy alloys are mainly prepared by vacuum arc melting and casting. However, due to the slow cooling rate of such methods, it is easy to produce component segregation, and it is not easy to form complex structural parts, which is not conducive to some practical application needs of high entropy alloys.

[0005] In view of this, additive manufacturing technology is the mainstream high-entropy alloy rapid prototyping technology that has emerged in recent years. Compared with traditional subtractive manufacturing processes, this additive manufacturing technology mainly uses the discrete accumulation forming principle, and uses high-energy beams to directly melt and accumulate materials into full-density, high-precision metal parts based on 3D three-dimensional model data. The main features of this technology are short part preparation time, insensitivity to complex structures, high material utilization and low manufacturing costs. It has great advantages for rapid manufacturing of high-entropy alloys with personalized structural topology and high forming accuracy requirements.

[0006] Functionally graded materials, with a continuous transition of microstructure or composition within a single component, are a new generation of innovative materials with an extraordinary ability to adapt to specific requirements or properties. Unlike traditional composite materials, functionally graded materials have well-defined interfaces between different regions, which helps to reduce stress concentrations in both mechanical and thermal aspects. Summary of the invention

[0007] As a further study on preparing a high entropy alloy layer with a functional gradient by additive technology, the present invention aims to provide a high entropy alloy layer component with relatively good hardness and wear resistance. The present invention also provides a method for preparing the high entropy alloy layer component.

[0008] In an embodiment of the present invention, a first aspect provides a high entropy alloy layer component, comprising a substrate and a cladding layer deposited on the surface of the substrate by laser cladding, wherein the cladding layer is a high entropy alloy layer;

[0009] The high entropy alloy layer includes five layers deposited in sequence, and the hardness of the five layers gradually increases from the inside to the outside;

[0010] Each layer has at least two sub-layers. The sub-layers contained in the same layer are made of the same material, and the next sub-layer is formed after one sub-layer is formed and stabilized.

[0011] Optionally, the number of sub-layers each layer has is three.

[0012] Optionally, the thickness of the outermost layer and the second outermost layer is no more than 5 mm.

[0013] Optionally, the thickness of the five layers gradually decreases from the inside to the outside.

[0014] Optionally, the high entropy alloy materials of the five layers from inside to outside are: FeCrCoNi, FeCrCoNiMo0.5, FeCrCoNiMo0.5W0.25, FeCrCoNiMo0.5W0.5 and FeCrCoNiMo0.5W0.75.

[0015] In an embodiment of the present invention, a method for preparing a high entropy alloy layer component is provided, which is used for preparing the high entropy alloy layer component of the first aspect. The preparation method comprises the following steps:

[0016] 1) Cleaning: cleaning and drying the surface of the substrate on which the high entropy alloy layer is to be prepared;

[0017] 2) Deposition: In the laser additive system, the selected high entropy alloy powder is sequentially deposited to form five deposition layers;

[0018] Each deposition layer has at least two sub-layers, and during the deposition process, the deposition of the next sub-layer must be completed and stabilized after the previous sub-layer has been deposited.

[0019] Optionally, the stabilization means that after the current sublayer is deposited, it is cooled to a temperature below 0.45 times the melting point of the deposited high entropy alloy powder, and not less than 0.3 times.

[0020] Optionally, according to the molar ratio of the components of the corresponding high entropy alloy, the components are put into a ball mill for uniform mixing after weighing, and then dried to be used as raw material powder for the laser additive system.

[0021] Optionally, in the cleaning step, the surface of the high entropy alloy to be prepared is first mechanically polished using sandpaper, then placed in an ultrasonic cleaner, cleaned using alcohol as an organic solvent, and further cleaned using deionized water and then dried.

[0022] Optionally, the process parameters of the laser additive manufacturing are:

[0023] The laser spot shape is circular, the powder feeding rate is 0.4L / min, the spot diameter is 2mm, the overlap rate is 40%, and the scanning speed is 300mm / min.

[0024] In an embodiment of the present invention, the prepared high entropy alloy layer has multiple high entropy alloy layers, and the hardness increases from the inside to the outside. Based on the gradient change of this hardness, it can adapt to application environments such as heavy loads. And each high entropy alloy layer has at least two sub-layers, which can make the corresponding high entropy alloy layer structure more stable and have a better transition effect overall. In addition, the wear resistance of the prepared high entropy alloy layer with five layers is also relatively good. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1a Schematic diagram of the cross-sectional structure of a high entropy alloy layer component in one embodiment (processing state).

[0026] Figure 1b This is the microscopic morphology of high entropy alloy powder under an electron microscope.

[0027] Figure 1c This is the order in which the functional layers of the high entropy alloy layer are formed.

[0028] Figure 2a This is a metallographic microscope photograph of the top of the sample cut in one embodiment.

[0029] Figure 2b and Figure 2c This is a metallographic microscope photograph of the middle portion of a sample cut in one embodiment.

[0030] Figure 2d The figure is a metallographic microscope photograph of the bottom of the sample cut in one embodiment.

[0031] Figure 3 FIG. 4 is a compressive engineering stress-strain curve of a sample in an embodiment.

[0032] Figure 4 FIG. 4 is a hardness distribution curve of a sample in an embodiment (along the construction direction).

[0033] Figure 5 This is a comparison diagram of the friction system-friction time curve between the sample and the substrate in an embodiment.

[0034] Figure 6 This is a comparison chart of the wear rates of the sample and the substrate in one embodiment.

[0035] In the figure: 1. substrate, 2. high entropy alloy layer, 3. protective gas, 4. powder. Implementation

[0036] According to the general definition of high entropy alloys, in the embodiments of the present invention, if the content of each component of the relevant high entropy alloy is not defined, it is expressed as an equal molar ratio, such as FeCrCoNi; if a superscript is used for marking, it indicates the amount (molar fraction) of the corresponding component alone, such as FeCrCoNiMo 0.5 , and the remaining components are in equal molar ratios. This is consistent with the general definition of high entropy alloys and can be correctly understood by those skilled in the art.

[0037] For continuous production, the relevant high entropy alloy powder is a high entropy alloy powder with a good ratio, and it can also be prepared and used immediately, depending on the process arrangements of different companies. However, it should be noted that the improvement direction of the present invention is not the improvement of the high entropy alloy itself, but the high entropy alloy layer and the preparation method of the high entropy alloy layer. Therefore, the high entropy alloy itself will not be described in detail.

[0038] In addition, it should be known that for continuous production on a production line, high entropy alloy powder is usually canned and fed by, for example, a powder feeding mechanism. Since it does not involve the improvements of the present invention, it will not be described in detail here.

[0039] If the high entropy alloy powder is damp, it will affect the uniformity of powder feeding and even block the pipeline. Of course, for a small amount of single-piece or small-batch production, the corresponding high entropy alloy powder can be dried after mixing evenly.

[0040] Therefore, for example, for sample production or small batch production, it can be prepared and used immediately, for example, using an electronic balance to weigh and prepare mixed powders of different atomic percentages (molar ratios). In one embodiment, five high entropy alloy powders are prepared, specifically FeCrCoNi, FeCrCoNiMo 0.5 、FeCrCoNiMo 0.5 W 0.25 、FeCrCoNiMo 0.5 W 0.5 and FeCrCoNiMo 0.5 W 0.75 From the perspective of alloy hardness, the five powders in the text sequence increase in sequence, as shown in Figure 1a In the figure, under the same process conditions, from the perspective of hardness, the deposited FeCrCoN high entropy alloy layer is located in the innermost layer, and forms a metallurgical connection with the substrate 1. The other layers are deposited in sequence to form Figure 1aThe high entropy alloy layer 2 having five layers shown in the figure has five layers. The high entropy alloy layer 2 formed by the laser cladding process has five layers. The hardness between the layers changes gradually from the inside to the outside, specifically, the gradient gradually increases. This gradient increase can make the high entropy alloy layer 2 have better toughness as a whole, is not easy to produce dislocations, and has better wear resistance.

[0041] In order to improve the verifiability, the following processing methods are provided for reference by technicians in this field. First, how to mix the high entropy alloy powder evenly is because the high entropy alloy powder components are relatively large. If the mixing is uneven, for example, the properties of the single metal phase in the local part of the prepared high entropy alloy layer 2 are relatively obvious, which affects the overall performance of the high entropy alloy layer 2. Therefore, after preparing a high entropy alloy powder, the high entropy alloy powder is placed in a ball mill for mixing for no less than 4 hours, preferably 5 hours, to ensure that the high entropy alloy powder can be fully mixed and the components are evenly dispersed.

[0042] When mixing in a ball mill, grinding balls made of GCr15 were used, the ratio of grinding balls to high entropy alloy powder was 3:1 (mass ratio), and the ball mill speed was 200 r / min.

[0043] It is even more necessary to solve the moisture absorption problem when preparing and using the powder immediately. Therefore, the high entropy alloy powder needs to be dried after being evenly mixed. For example, the evenly mixed high entropy alloy powder can be placed in a drying oven at 120°C for 4 hours to remove moisture, thereby ensuring its dryness.

[0044] like Figure 1a The powder 4 and high entropy alloy powder in the medium generally need to be transported through pipelines. The relatively dry powder 4 has good fluidity and relatively good feeding uniformity.

[0045] The above-mentioned five high-entropy alloys are an example of a high-entropy alloy combination. It should be noted that high-entropy alloys are easy to form metallurgical connections, which is independent of the type of high-entropy alloy. Based on the concept of gradually improving hardness, the combination of five high-entropy alloys determined by technicians in this field should fall within the scope of protection of the present invention.

[0046] For the convenience of description, unless otherwise specified, the above five high entropy alloy powders are used as raw material powders for preparing the high entropy alloy layer 2, and Q235 steel is used as the matrix for explanation.

[0047] It should be known that with the help of a laser additive system (a relatively mature process equipment, which will not be described in detail here), it is a common method in this field to deposit different high entropy alloy functional layers (hereinafter referred to as layers) layer by layer. The layers formed are metallurgical connections based on laser cladding, and have high bonding strength.

[0048] Figure 1bAn electron microscope image of a high entropy alloy powder is shown. The particle size is relatively uniform, the dispersion is relatively good in a dry state, and it is easy to be transported through a pipeline. It is suitable as a raw material powder for a laser additive system.

[0049] In order to ensure the adhesion between the high entropy alloy layer 2 and the substrate 1 (for example, a steel substrate with a grade of Q235), the substrate 1 is pretreated, mainly to remove the oxide layer and dirt on the surface of the substrate. First, sandpaper, such as 200-mesh sandpaper, is used to polish the surface of the group 1, and then anhydrous alcohol is used for ultrasonic cleaning (the process equipment is an ultrasonic cleaning instrument).

[0050] Furthermore, a fiber laser additive manufacturing system with a maximum output power of 2000W is used to deposit the powder 4 on the substrate 1. The deposition is carried out under a protective atmosphere, and the protective gas is an inert gas, preferably argon. Since these are inherent configurations of the laser additive system, they will not be described in detail here.

[0051] Figure 1a The positional relationship of the five layers is shown. In the figure, the side close to the substrate 1 is the inner side, and the side far from the substrate 1 is the outer side. It can generally be described as up and down. The one at the bottom is the bottommost side, and the other side is the topmost layer.

[0052] Figure 1c The forming sequence of the five layers is shown, the vertical arrows indicate the deposition from the inside to the outside, and the oblique arrows indicate the way the laser spot scans back and forth.

[0053] First, FeCrCoNi powder was deposited, and the working parameters of the laser were selected as follows: power of 1000 W, circular spot shape with a diameter of 2 mm, corresponding powder feeding rate of 0.4 L / min, spot overlap rate of 30%, and scanning speed of 300 mm / min.

[0054] After depositing one sub-layer, the deposition is continued according to the working parameters, and three sub-layers are deposited in total. The total layer thickness of the three sub-layers is controlled between 6 mm and 8 mm.

[0055] Then, FeCrCoNiMo0.5 powder was deposited, the laser power was selected to be 1300W, the spot shape was circular, the spot diameter was 2mm, the spot overlap rate was 40%, the corresponding powder feeding rate was 0.3L / min, the scanning speed was 300mm / min, and after depositing one sub-layer, the deposition was continued according to this working parameter, and a total of three sub-layers were deposited. The total layer thickness of the three sub-layers was controlled between 4mm and 6mm.

[0056] Then, FeCrCoNiMo0.5W0.25 powder was deposited, the laser power was selected to be 1300W, the spot shape was circular, the spot diameter was 2mm, the spot overlap rate was 40%, the corresponding powder feeding rate was 0.3L / min, the scanning speed was 300mm / min, and after depositing one sublayer, the deposition was continued according to this working parameter, and a total of three sublayers were deposited. The total layer thickness of the three sublayers was controlled between 4mm and 6mm.

[0057] Then, FeCrCoNiMo0.5W0.5 powder was deposited, the laser power was selected to be 1300W, the spot shape was circular, the spot diameter was 2mm, the spot overlap rate was 50%, the corresponding powder feeding rate was 0.2L / min, the scanning speed was 300mm / min, and after depositing one sub-layer, the deposition was continued according to this working parameter, and a total of three sub-layers were deposited. The total layer thickness of the three sub-layers was controlled between 3mm and 5mm.

[0058] Finally, FeCrCoNiMo0.5W0.75 powder was deposited, the laser power was selected to be 1300W, the spot shape was circular, the spot diameter was 2mm, the spot overlap rate was 50%, the corresponding powder feeding rate was 0.2L / min, the scanning speed was 300mm / min, and after depositing one sub-layer, the deposition was continued according to this working parameter, and a total of three sub-layers were deposited. The total layer thickness of the three sub-layers was controlled between 3mm and 5mm.

[0059] From the above description, it can be seen that each layer contains three sub-layers. In other words, each high entropy alloy powder chooses to deposit three sub-layers because compared with depositing independent functional layers, the microstructure of the same powder will be more stable, and a better transition effect can be achieved overall, and the material will obtain better mechanical properties. Through experimental comparison, the compressive strength of the gradient functional material deposited with three sub-layers of each powder can reach 2041MPa, and the hardness can reach 892HV, while the compressive strength of the gradient functional material deposited with a single layer of each powder is 1562MPa, and the hardness is 755HV. In addition, depositing three sub-layers can better build up the thickness of the functional gradient material to meet the actual working conditions. In other words, if the thickness of a single layer is too large, the heat penetration efficiency is relatively low.

[0060] There is a scanning speed as mentioned above. After one sub-layer is formed, another sub-layer will quickly cool to a relatively low temperature. It should be known that the larger the thermal step (the temperature difference between the object temperature and the ambient temperature), the faster the object loses temperature. Usually, the next sub-layer can be deposited without separate cooling.

[0061] In addition, it has been found through experiments that if the temperature drops too quickly after the deposition of a sublayer, the amplitude of thermal alternation will be too large when the next sublayer is deposited, affecting the overall mechanical properties, specifically thermal brittleness. Therefore, in a preferred embodiment, it is necessary to prevent the object (substrate 1 or a workpiece containing other functional layers) from losing temperature too quickly. It is very easy for technicians in this field to adjust the ambient temperature based on the temperature at the beginning of the current sublayer after depositing a sublayer, so as to control the amplitude of thermal alternation. It is preferred to avoid the object's starting temperature after depositing a sublayer being lower than 0.3 times its melting point, and preferably not higher than 0.45 times its melting point.

[0062] Furthermore, although different total thickness materials can be obtained by changing the layer thickness corresponding to each high entropy alloy powder, the thickness of the fourth and fifth layers of the high entropy alloy layer 2 (numbered from the inside to the outside, or numbered according to the construction direction) should not be too large. As mentioned above, when the single layer thickness of the fourth and fifth layers exceeds 5 mm, cracks will appear on the top of the functional gradient material. This is because Mo and W have high melting points, high thermal conductivity and brittleness, and are relatively difficult to additively manufacture. Cracks have always been and remain one of the most challenging problems in this field.

[0063] A large amount of Mo and W added to a high entropy alloy will produce a large amount of brittle second-phase intermetallic compounds. If the deposited layer is too thick and there are too many brittle second-phase intermetallic compounds, the material will crack, seriously affecting the mechanical properties of the material. This is because during the DED process, rapid heating and continuous heating and cooling cycles produce a large number of liquefaction cracks and residual stresses, which lead to the generation of cracks in the material, and the cracks will extend along the high-angle grain boundaries of the material. Therefore, the fourth and fifth layers are deposited as thick as possible. In addition, the temperature at the beginning of the sub-layer after the deposition of the included sub-layer is better controlled to reduce the impact of thermal alternation temperature difference.

[0064] Next, the prepared workpiece is inspected, specifically, the workpiece having the high entropy alloy layer 2 generated after the deposition is completed is inspected. The portion of the workpiece including the high entropy alloy layer 2 is cut into 10 mm×10 mm samples using a wire cutting machine for the convenience of the subsequent test.

[0065] The selected first group of samples were placed in an ultrasonic cleaner for cleaning, and the surfaces of the samples having the high entropy alloy layer 2 were polished in sequence using sandpaper ranging from 240 mesh to 2000 mesh from coarse to fine, and finally polished using a diamond polishing liquid through a polishing machine.

[0066] The polished sample was then chemically etched using aqua regia solution. The overall morphology of the cross section of the etched sample was observed using a metallographic microscope (OM).

[0067] Then, a microcomputer-controlled electronic universal testing machine was used to perform compression tests on the substrate 1 and the high entropy alloy layer 2 in the second group of samples.

[0068] The cross-sectional hardness of the third group of specimens was measured from the substrate to the top of the material using a Vickers hardness tester (402MVD) with a load of 500 g and a duration of 15 s.

[0069] Furthermore, the fourth group of samples and substrate 1 were placed on a RTEC-MFT-50 testing machine in a reciprocating friction and wear testing machine to test wear resistance. The friction and wear test parameters were reciprocating frequency: 4 Hz, applied load: 50 N, temperature: room temperature, stroke: 8 mm, and time: 30 min.

[0070] Performance analysis: Figure 2a~2d The results are clearly visible, and it can be seen that the high entropy alloy functional gradient material manufactured by laser additive manufacturing is of good quality, with a dense microstructure and no obvious pores and cracks. Figure 2a As shown in Figure 2, some second phase intermetallic compounds are precipitated in the top region of the high entropy alloy functional gradient material. Figure 2b As shown in Figure 2-c, epitaxially grown columnar crystals, slender dendrites and dense equiaxed crystals are the main microstructures in the middle of the high entropy alloy functional gradient material. Figure 2d As shown, a planar crystal structure growing in a plane is generated between the matrix and the high entropy alloy functional gradient material. The appearance of the planar crystal proves that a good metallurgical bonding is formed between the matrix and the high entropy alloy functional gradient material.

[0071] Figure 3 It is the compressive engineering stress-strain curve of the sample and the substrate 1. Since the substrate is plastic steel, compression fracture will not occur and the compression curve will not decrease. Compared with the substrate 1, the compressive strength of the high entropy alloy layer 2 formed by the high entropy alloy functional gradient material is significantly better. The compressive fracture stress and fracture strain of the high entropy alloy functional gradient material are 2041±45MPa and 21.6±0.9%.

[0072] Figure 4 This is the hardness distribution curve of the sample prepared by high entropy alloy functional gradient material along the construction direction. The hardness of high entropy alloy functional gradient material shows a significant gradient change, indicating that the design of high entropy alloy functional gradient material is reasonable in terms of hardness improvement. The hardness shows a continuous upward process, reaching 892.5HV0.3 at the top of the high entropy alloy functional gradient material, which is 4.95 times that of the base material Q235.

[0073] The results of friction and wear tests can be found in Figure 5 , Figure 6 .Depend on Figure 5As shown in FIG. 1 , at room temperature, the friction coefficient of the high entropy alloy layer 2 prepared from the high entropy alloy functional gradient material is much lower than the friction coefficient of the substrate Q235. Figure 6 As shown, the wear rate of the high entropy alloy layer 2 prepared by the high entropy alloy functional gradient material is significantly lower than that of the substrate 1, and the wear rate at room temperature is only 25.99% of that of the substrate 1. The size of the wear rate can indirectly reflect the quality of wear resistance, which also reflects the excellent wear resistance of the high entropy alloy functional gradient material.

[0074] The excellent mechanical properties of high entropy alloy functional gradient materials come from: (1) The atomic radius of Mo and W is much larger than that of Co, Cr, Fe and Ni. When they enter the lattice to form a substitutional solid solution, they will cause a lattice distortion effect, enhance the solid solution strengthening effect, and increase the internal energy and micro stress of the material. They also hinder the slip deformation of dislocations, thereby increasing the strength of high entropy alloy functional gradient materials. (2) The large amount of W and Mo added promotes the grain refinement of high entropy alloy functional gradient materials, and grain refinement strengthening also greatly improves the strength of high entropy alloy functional gradient materials. (3) High concentrations of W and Mo promote the formation of μ-phase and σ-phase intermetallic compounds. μ-phase and σ-phase are hard phases that can effectively inhibit dislocation movement and increase the resistance to dislocation slip. Dislocations are entangled near the hard phase during deformation. The more hard phase content there is, the stronger the resistance to dislocations. Therefore, second phase strengthening plays an important role in improving the compressive strength and wear resistance of high entropy alloy functional gradient materials. (4) During the laser additive manufacturing process, local melting and layer-by-layer addition will cause the high-entropy alloy functional gradient material to be continuously remelted and tempered, reducing the interface hardness between the layers. In addition, due to the large thermal gradient in the laser additive manufacturing process, a large amount of residual stress will be introduced. While ensuring that the high-entropy alloy functional gradient material has no microcracks, appropriate residual stress will also improve the strength of the high-entropy alloy functional gradient material. (5) The top of the high-entropy alloy functional gradient material has a very high dislocation density. The higher the dislocation density, the more displacements there are in the crystal, and the larger the inherent stress field of the crystal, thereby increasing the strength of the high-entropy alloy functional gradient material.

Claims

1. A high entropy alloy layer component, comprising a substrate and a cladding layer deposited on the surface of the substrate by laser cladding, It is characterized in that The cladding layer is a high entropy alloy layer; The high entropy alloy layer includes five layers deposited in sequence, and the hardness of the five layers gradually increases from the inside to the outside; Each layer has at least two sub-layers, and the sub-layers contained in the same layer are made of the same material, and the next sub-layer is formed after one sub-layer is formed and stabilized; The thickness of the five layers from inside to outside are 6mm-8mm, 4mm-6mm, 4mm-6mm, 3mm-5mm, and 3mm-5mm.

2. The high entropy alloy layer according to claim 1, It is characterized in that The number of sublayers each layer has is three.

3. The high entropy alloy layer according to claim 1, It is characterized in that The high entropy alloy materials of the five layers from inside to outside are: FeCrCoNi, FeCrCoNiMo 0.5 、FeCrCoNiMo 0.5 W 0.25 、FeCrCoNiMo 0.5 W 0.5 and FeCrCoNiMo 0.5 W 0.75 .

4. A method for preparing a high entropy alloy layer component, used for preparing the high entropy alloy layer component according to any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: 1) Cleaning: cleaning and drying the surface of the substrate on which the high entropy alloy layer is to be prepared; 2) Deposition: In the laser additive system, the selected high entropy alloy powder is sequentially deposited to form five deposition layers; Each deposition layer has at least two sub-layers, and during the deposition process, the deposition of the next sub-layer must be completed and stabilized after the previous sub-layer is deposited; The stability means that after the current sub-layer is deposited, it is cooled to a temperature below 0.45 times the melting point of the deposited high entropy alloy powder, and not less than 0.3 times; The thickness of the five layers from inside to outside are 6mm-8mm, 4mm-6mm, 4mm-6mm, 3mm-5mm, and 3mm-5mm.

5. The preparation method according to claim 4, It is characterized in that According to the molar ratio of the components of the corresponding high entropy alloy, the mixture is put into a ball mill for uniform mixing after weighing, and then dried to be used as the raw material powder of the laser additive system.

6. The preparation method according to claim 4, It is characterized in that In the cleaning step, the surface of the high entropy alloy to be prepared is first mechanically polished using sandpaper, then placed in an ultrasonic cleaner, cleaned using alcohol as an organic solvent, and further cleaned using deionized water and then dried.

7. The preparation method according to claim 4, It is characterized in that The process parameters of the laser additive manufacturing are: The laser spot shape is circular, the powder feeding rate is 0.4L / min, the spot diameter is 2mm, the overlap rate is 40%, and the scanning speed is 300mm / min.