A method for preparing graphene oxide thin films
By coating a graphene oxide dispersion onto an absorbent sponge and then drying it, a graphene oxide film is prepared, solving the problem of slow production speed of large-diameter films in existing technologies. This enables rapid film formation and large-scale production, making it suitable for various application scenarios.
Patent Information
- Application Number
- CN202310699603.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-06-13
Smart Images

Figure CN116675222B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of graphene film materials, and more particularly to a method for preparing graphene oxide films. Background Technology
[0002] Graphene oxide is a single-layer material peeled off from graphene oxide. It is a graphene derivative with special structure and properties. Its surface is covered with a large number of functional groups such as hydroxyl, carboxyl and epoxy groups, which gives it a certain degree of hydrophilicity.
[0003] Due to the needs of engineering applications, graphene oxide nanosheets are typically assembled into graphene oxide thin films using various liquid-phase film-forming techniques for applications in electrochemical catalysis, impurity separation, and sensor devices. Common liquid-phase film-forming methods include vacuum filtration and spin coating.
[0004] Vacuum filtration is a commonly used separation technique, typically used to separate solid particles or sheet-like masses from solutions. Its basic principle is to use negative pressure to force the solution through a filter membrane, isolating the solid particles or sheets on the membrane to form a thin film. However, because the size of the vacuum filtration film is related to the diameter of the filtration flask and the film formation time is relatively long, large-scale production of thin films is difficult. Another method, spin coating, involves coating a liquid material onto a rotating substrate surface, using centrifugal force to uniformly distribute the solution on the surface to form a thin film, followed by heating and annealing to create a dense film structure. However, spin-coating films are usually limited by the substrate, making it impossible to produce large films. Therefore, developing a novel and rapid method for preparing large-diameter graphene oxide thin films is particularly urgent. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing graphene oxide films. This invention provides a fast film formation rate for preparing graphene oxide films and enables large-scale production of graphene oxide films.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0007] This invention provides a method for preparing graphene oxide thin films, comprising the following steps:
[0008] The graphene oxide dispersion was coated onto a microfiltration membrane with an absorbent sponge placed underneath and then filtered. The resulting graphene oxide wet membrane was dried to obtain the graphene oxide film.
[0009] Preferably, the concentration of the graphene oxide dispersion is 1–5 mg / mL.
[0010] Preferably, the pore size of the microfiltration membrane is 0.1 to 5 μm.
[0011] Preferably, the microfiltration membrane includes one or more of the following: mixed cellulose membrane, polytetrafluoroethylene membrane, nylon membrane, polyvinylidene fluoride membrane, polyethersulfone membrane, and polypropylene membrane.
[0012] Preferably, the mixed cellulose filter membrane comprises cellulose diacetate and cellulose nitrate;
[0013] The mass ratio of cellulose diacetate to cellulose nitrate is 1:0.25 to 1.5.
[0014] Preferably, the absorbent sponge includes one or more of wood pulp sponge, polyvinyl alcohol sponge, polyurethane sponge, and melamine sponge.
[0015] Preferably, the porosity of the absorbent sponge is 70-90%.
[0016] Preferably, the method for preparing the polyvinyl alcohol sponge includes the following steps:
[0017] Polyvinyl alcohol, polyurethane prepolymer, water, and catalyst are mixed and subjected to a crosslinking reaction to obtain the polyvinyl alcohol sponge.
[0018] Preferably, the water content of the graphene oxide wet film is 75-98 wt%.
[0019] Preferably, the drying includes natural evaporation and / or heat drying;
[0020] The heating and drying temperature is 30–100°C, and the time is 30–90 min.
[0021] This invention provides a method for preparing a graphene oxide film, comprising the following steps: coating a graphene oxide dispersion onto a microfiltration membrane with an absorbent sponge placed underneath for percolation; drying the resulting wet graphene oxide membrane to obtain the graphene oxide film. In this invention, after the graphene oxide dispersion is drop-coated onto a filter membrane with an absorbent sponge placed underneath, due to the capillary action between the solid and liquid and the surface tension of the liquid, water molecules in the solution rapidly permeate the filter membrane and are absorbed by the hydrophilic sponge, thereby accelerating the film formation rate of the graphene oxide film and enabling large-scale preparation of graphene oxide films. Attached Figure Description
[0022] Figure 1 This is a flowchart illustrating the preparation process of the graphene oxide film according to an embodiment of the present invention.
[0023] Figure 2 This is a micrograph of graphene oxide provided in Example 1 of the present invention;
[0024] Figure 3 This is a surface morphology diagram of the graphene oxide film provided in Embodiment 1 of the present invention;
[0025] Figure 4 This is a cross-sectional view of the graphene oxide film provided in Embodiment 2 of the present invention;
[0026] Figure 5 This is a physical image of the graphene oxide film provided in Embodiment 2 of the present invention;
[0027] Figure 6 This is a graph showing the relationship between solution concentration and film formation time provided in Example 3 of the present invention;
[0028] Figure 7 This is a graph showing the relationship between sponge thickness and film formation time provided in Embodiment 4 of the present invention;
[0029] Figure 8 This is a graph showing the pore size and film formation time of the filter membrane provided in Embodiment 4 of the present invention. Detailed Implementation
[0030] This invention provides a method for preparing graphene oxide thin films, comprising the following steps:
[0031] The graphene oxide dispersion was coated onto a microfiltration membrane with an absorbent sponge placed underneath and then filtered. The resulting graphene oxide wet membrane was dried to obtain the graphene oxide film.
[0032] In this invention, the preparation method of the graphene oxide dispersion preferably includes the following steps:
[0033] Graphene oxide was dispersed in water to obtain the graphene oxide dispersion.
[0034] In this invention, the concentration of the graphene oxide dispersion is preferably 1-5 mg / mL, more preferably 2-4 mg / mL.
[0035] In this invention, the method for preparing the graphene oxide preferably includes the following steps:
[0036] Natural graphite, sodium nitrate, and concentrated sulfuric acid are mixed to obtain a mixture;
[0037] The mixture was mixed with potassium permanganate to carry out a first oxidation reaction to obtain the oxidation reaction product;
[0038] The oxidation reaction product was diluted with water and then mixed with hydrogen peroxide solution to carry out a second oxidation reaction, yielding graphene oxide.
[0039] This invention involves mixing natural graphite, sodium nitrate, and concentrated sulfuric acid to obtain a mixture. In this invention, the preferred mass ratio of natural graphite, sodium nitrate, and concentrated sulfuric acid is 1 g:1 g:30 mL; the preferred mass concentration of the concentrated sulfuric acid is 80-98%. In this invention, the mixing is preferably carried out under ice bath conditions. Sodium nitrate and concentrated sulfuric acid create a mildly reactive strong acid environment because if sodium nitrate is not added and sulfuric acid is used directly, the reaction will be violent and release a large amount of heat when water is added subsequently. The role of concentrated sulfuric acid is to disrupt the conjugated structure of graphite. Concentrated sulfuric acid acts as an intercalating agent, entering the interlayer of graphite sheets to cause graphite expansion, facilitating subsequent oxidative exfoliation; furthermore, concentrated sulfuric acid can acidify potassium permanganate, enhancing its oxidizing properties.
[0040] After obtaining the mixture, the present invention mixes the mixture with potassium permanganate to carry out a first oxidation reaction to obtain the oxidation reaction product. In the present invention, the mass of the potassium permanganate is preferably 5-20% of the mass of the mixture, more preferably 12-16%. The first oxidation reaction is preferably carried out for 3-6 hours, and preferably under stirring conditions. The oxidation reaction between natural graphite intercalated with concentrated sulfuric acid and potassium permanganate introduces oxygen-containing functional groups (such as hydroxyl groups, ketone groups, ether bonds, etc.) into the graphite interlayer, thereby weakening the van der Waals forces between the layers to obtain graphite oxide.
[0041] After obtaining the oxidation reaction product, the present invention dilutes the oxidation reaction product with water and mixes it with hydrogen peroxide solution to carry out a second oxidation reaction to obtain graphene oxide. In the present invention, the mass ratio of water to the oxidation reaction product is preferably ≥2.
[0042] In this invention, the mass of the hydrogen peroxide solution is preferably 2-5% of the total mass of the oxidation reaction products and water, more preferably 3-4%. The mass content of the hydrogen peroxide solution is preferably 99.5-99.8%. In the reduction reaction, hydrogen peroxide reacts with unreacted potassium permanganate, reducing the heptavalent manganese ions in the potassium permanganate to divalent manganese ions, which facilitates processing.
[0043] Following the second oxidation reaction, the present invention preferably further involves sequentially filtering, washing, centrifuging, and drying the product of the second oxidation reaction to obtain graphene oxide. The present invention does not impose any particular limitations on the filtration, centrifugation, and washing processes; any method well-known to those skilled in the art can be used to remove residual acid and impurities. Specifically, in the embodiments of the present invention, impurities are removed by filter paper filtration and washed with a large amount of ultrapure water. Finally, the impurities are separated by centrifugation at 1000 rpm and dried at 80°C for 5 hours.
[0044] The present invention does not have any special requirements on the amount of the graphene oxide dispersion; it can be determined according to the thickness and size of the target graphene oxide film.
[0045] In this invention, the pore size of the microfiltration membrane is preferably 0.1–5 μm, more preferably 0.2–0.4 μm; the filter membrane includes one or more of the following: mixed cellulose filter membrane, polytetrafluoroethylene filter membrane, nylon filter membrane, polyvinylidene fluoride filter membrane, polyethersulfone filter membrane, and polypropylene filter membrane, more preferably a mixed cellulose filter membrane. This invention does not impose any special limitation on the size of the filter membrane; it can be determined based on the size of the target graphene oxide film.
[0046] In this invention, the mixed cellulose filter membrane preferably comprises cellulose diacetate and cellulose nitrate; the mass ratio of cellulose diacetate to cellulose nitrate is 1:0.25 to 1.5.
[0047] In this invention, the absorbent sponge preferably includes one or more of wood pulp sponge, polyvinyl alcohol sponge, polyurethane sponge, and melamine sponge, more preferably polyvinyl alcohol sponge. In this invention, the absorbency of the absorbent sponge is preferably more than 10 times its own weight. In this invention, the porosity of the absorbent sponge is preferably 70-90%, more preferably 80-85%.
[0048] In this invention, the method for preparing the polyvinyl alcohol sponge includes the following steps:
[0049] Polyvinyl alcohol, polyurethane prepolymer, water, and catalyst are mixed and subjected to a crosslinking reaction to obtain the polyvinyl alcohol sponge.
[0050] In this invention, the mixing preferably includes: dissolving polyvinyl alcohol in water to obtain a polyvinyl alcohol solution; and mixing the polyvinyl alcohol solution with a polyurethane prepolymer and a catalyst.
[0051] In this invention, the dissolution temperature is preferably 100°C, and the dissolution time is preferably 1 hour; the dissolution is preferably carried out under magnetic stirring conditions, and the magnetic stirring speed is preferably 300 r / min. The concentration of the polyvinyl alcohol solution is preferably 100–300 mg / mL, more preferably 150–250 mg / mL, and even more preferably 180–200 mg / mL; the mass of the polyurethane prepolymer is preferably 10–20% of the mass of the polyvinyl alcohol solution, more preferably 15–16%; the polyurethane prepolymer is obtained by reacting a polyol with a polyisocyanate. The molar ratio of the isocyanate group in the polyisocyanate to the hydroxyl group in the polyol is greater than 1; the end group of the polyurethane prepolymer is -NCO, and the mass content of NCO in the polyurethane prepolymer is preferably 5%. In this invention, the polyurethane prepolymer is preferably from LANXESS. BI7675.
[0052] The mass of the catalyst is preferably 1-3% of the mass of the polyvinyl alcohol solution, more preferably 2-2.5%; the catalyst preferably includes one or more of stannous triethanolamine octoate, dibutyltin dilaurate and N-methylmorpholine.
[0053] In this invention, the mixing temperature is preferably 60–80°C, more preferably 80–90°C. The mixing is preferably carried out under stirring conditions. The stirring speed is preferably 450–1000 r / min, and the stirring time is preferably 2–8 min.
[0054] In this invention, the crosslinking reaction is preferably carried out in a mold. The temperature of the crosslinking reaction is preferably 110–130°C, more preferably 120–125°C; the time is preferably 3–5 h, more preferably 4–4.5 h. During the crosslinking reaction, the polyurethane prepolymer crosslinks with polyvinyl alcohol to form a network structure.
[0055] In this invention, the filtration time is preferably 12-40 min, more preferably 20-30 min; the water content of the graphene oxide wet film is 75-98 wt%; the graphene oxide wet film is non-flowable; the drying includes natural evaporation and / or heating drying; the heating drying temperature is preferably 30-50°C, more preferably 40-45°C, and the time is preferably 1-2 h, more preferably 1.2-1.6 h.
[0056] In this invention, the thickness of the graphene oxide film is preferably 10–50 μm, more preferably 20–40 μm, and even more preferably 25–30 μm, and the roughness is preferably less than 1 μm. This invention does not impose any special limitations on the size of the graphene oxide film; it can be determined according to the target size. Specifically, in the embodiments of this invention, the width is 320 mm and the length is 1–3 m.
[0057] The preparation flow chart of the graphene oxide thin film in this embodiment of the invention is as follows: Figure 1 As shown. The filter membrane is laid flat on an absorbent sponge, and then the graphene oxide dispersion is drop-coated onto the filter membrane, followed by drying.
[0058] The following detailed description of the preparation method of the graphene oxide film provided by the present invention, in conjunction with the embodiments, should not be construed as limiting the scope of protection of the present invention.
[0059] The polyurethane prepolymer used in this embodiment of the invention is from LANXESS. BI7675.
[0060] Example 1
[0061] Add 10g of polyvinyl alcohol to a beaker and add 60mL of deionized water. Then place the beaker on a magnetic stirrer at 100℃ and stir at 300r / min for 1 hour to obtain a completely dissolved polyvinyl alcohol aqueous solution.
[0062] 10g of polyurethane prepolymer and 1g of stannous octoate were added to a polyvinyl alcohol aqueous solution to obtain a polyvinyl alcohol mixture. Then, the beaker was placed in an 80°C water bath and stirred for 2 minutes with a stirrer at 450 r / min. After stirring, the solution was poured into a mold and cured at 110°C for 3 hours. After curing, a polyvinyl alcohol hydrophilic sponge with a porosity of 60% was obtained.
[0063] Take 5g of natural graphite and 5g of sodium nitrate and place them in a beaker. Place the beaker in an ice bath and slowly add 150mL of 80% concentrated sulfuric acid while stirring constantly to disperse it evenly. Then add 15g of potassium permanganate and react for 3 hours. Add 700mL of deionized water, followed by dropwise addition of 20mL of 99.8% hydrogen peroxide solution. Filter the solution with filter paper to remove impurities and wash with plenty of ultrapure water. Finally, centrifuge at 1000rpm to separate impurities and dry at 80℃ for 5 hours to obtain layered graphene oxide powder. Figure 2 As shown.
[0064] A 1 mg / mL aqueous solution of graphene oxide was prepared. A microporous filter membrane (a mixed cellulose filter membrane made of nitrocellulose and cellulose acetate in a weight ratio of 6:4) with a pore size of 0.45 μm, a width of 320 mm, and a length of 1 m was placed on a 1 mm thick absorbent sponge. 1.5 L of the graphene oxide aqueous solution was scraped onto the microporous filter membrane. After standing for 40 min, a wet graphene oxide membrane with a water content of 96 wt% was obtained. The membrane was dried at 50 °C for 2 h. After drying, the graphene oxide membrane was peeled off from the filter membrane.
[0065] The surface morphology of the graphene oxide film in Example 1 was analyzed, and the results are as follows: Figure 3 As shown. By Figure 3 It can be seen that the surface roughness of the film is less than 1 μm and the thickness of the film is 10 μm.
[0066] Example 2
[0067] 10g of polyurethane prepolymer and 1g of stannous octoate were added to the polyvinyl alcohol aqueous solution of Example 1 to obtain a polyvinyl alcohol mixture. Then, the beaker was placed in a water bath at 80°C and stirred for 3 minutes with a stirrer at 600 r / min. After stirring, the solution was poured into a mold and cured at 110°C for 3 hours. After curing, a polyvinyl alcohol hydrophilic sponge with a porosity of 70% was obtained.
[0068] The graphene oxide powder prepared in Example 1 was mixed with plasma water to prepare a 2 mg / mL graphene oxide aqueous solution. A microporous filter membrane (a mixed cellulose filter membrane made of nitrocellulose and cellulose acetate in a weight ratio of 6:4) with a pore size of 1 μm, a width of 320 mm, and a length of 2 m was placed on a 2 mm thick absorbent sponge. 1.5 L of graphene oxide aqueous solution was scraped onto the microporous filter membrane. After standing for 35 min, a graphene oxide wet membrane with a water content of 91 wt% was obtained. The membrane was dried at 40 °C for 1.5 h. After drying, the graphene oxide membrane was peeled off from the filter membrane.
[0069] The cross-section of the graphene oxide film in Example 2 was analyzed, and the results are as follows: Figure 4 As shown. By Figure 4 It can be seen that the film is composed of stacked graphene oxide sheets, and the thickness of the film is 25 μm.
[0070] A physical image of the graphene oxide film in Example 2 is shown below. Figure 5 As shown.
[0071] Example 3
[0072] 10g of polyurethane prepolymer and 1g of stannous octoate were added to the polyvinyl alcohol aqueous solution of Example 1 to obtain a polyvinyl alcohol mixture. Then, the beaker was placed in a water bath at 80°C and stirred for 5 minutes with a stirrer at 800 r / min. After stirring, the solution was poured into a mold and cured at 110°C for 3 hours. After curing, a polyvinyl alcohol hydrophilic sponge with a porosity of 80% was obtained.
[0073] The graphene oxide powder prepared in Example 1 was mixed with plasma water to prepare a 3 mg / mL graphene oxide aqueous solution. A microporous filter membrane (a mixed cellulose filter membrane made of nitrocellulose and cellulose acetate in a weight ratio of 6:4) with a pore size of 3 μm, a width of 320 mm, and a length of 1 m was placed on a 3 mm thick absorbent sponge. 1.5 L of graphene oxide aqueous solution was scraped onto the microporous filter membrane. After standing for 23 min, a graphene oxide wet membrane with a water content of 84 wt% was obtained. The membrane was dried at 40 °C for 1 h. After drying, the graphene oxide membrane was peeled off from the filter membrane. The thickness of the membrane was 40 μm.
[0074] Example 4
[0075] 10g of polyurethane prepolymer and 1g of stannous octoate were added to the polyvinyl alcohol aqueous solution of Example 1 to obtain a polyvinyl alcohol mixture. Then, the beaker was placed in a water bath at 80°C and stirred for 8 minutes with a stirrer at 1000 r / min. After stirring, the solution was poured into a mold and cured at 110°C for 3 hours. After curing, a polyvinyl alcohol hydrophilic sponge with a porosity of 90% was obtained.
[0076] The graphene oxide powder prepared in Example 1 was mixed with plasma water to prepare a 4 mg / mL graphene oxide aqueous solution. A microporous filter membrane (a mixed cellulose filter membrane made of nitrocellulose and cellulose acetate in a weight ratio of 6:4) with a pore size of 5 μm, a width of 320 mm, and a length of 1 m was placed on a 4 mm thick absorbent sponge. 1.5 L of graphene oxide aqueous solution was scraped onto the microporous filter membrane. After standing for 12 min, a graphene oxide wet membrane with a water content of 79 wt% was obtained. The membrane was dried at 40 °C for 40 min. After drying, the graphene oxide membrane was peeled off from the filter membrane. The thickness of the membrane was 50 μm. The thicker the absorbent sponge, the faster the film formation speed.
[0077] The film formation rates of Examples 1-4 were analyzed, and the results are as follows: Figures 6-8 As shown. By Figures 6-8 It can be seen that the film-forming speed of graphene oxide aqueous solutions with different concentrations is different; the thicker the water-absorbing sponge, the faster the film-forming speed.
[0078] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a graphene oxide thin film, characterized in that, Includes the following steps: The graphene oxide dispersion was coated onto a microfiltration membrane with an absorbent sponge placed underneath and then filtered. The resulting graphene oxide wet membrane was dried to obtain the graphene oxide film. The concentration of the graphene oxide dispersion is 1~5 mg / mL; The pore size of the microfiltration membrane is 0.1~5μm; The microfiltration membrane includes one or more of the following: mixed cellulose membrane, polytetrafluoroethylene membrane, nylon membrane, polyvinylidene fluoride membrane, polyethersulfone membrane, and polypropylene membrane; The absorbent sponge includes one or more of wood pulp sponge, polyvinyl alcohol sponge, polyurethane sponge, and melamine sponge; The porosity of the absorbent sponge is 70-90%.
2. The preparation method according to claim 1, characterized in that, The mixed cellulose filter membrane comprises cellulose diacetate and cellulose nitrate; The mass ratio of cellulose diacetate to cellulose nitrate is 1:0.25~1.
5.
3. The preparation method according to claim 1, characterized in that, The preparation method of the polyvinyl alcohol sponge includes the following steps: Polyvinyl alcohol, polyurethane prepolymer, water, and catalyst are mixed and subjected to a crosslinking reaction to obtain the polyvinyl alcohol sponge.
4. The preparation method according to claim 1, characterized in that, The water content of the graphene oxide wet film is 75~98wt%.
5. The preparation method according to claim 1 or 4, characterized in that, The drying process includes natural evaporation and / or heated drying; The heating and drying temperature is 30~100℃, and the time is 30~90min.
Citation Information
Patent Citations
Preparation method of reduction graphene oxide heat-conducting film
CN104030275A
Flexible thin film attaching method, flexible thin film stripping method, flexible substrate preparation method and base substrate
CN105690974A