A method for firing porcelain blanks to prevent head-turning at high temperature
By finely controlling the kiln parameters at different stages of the kiln to ensure that the temperature of the upper part is lower than the temperature of the lower part, the problem of burning ends of the porcelain blank is solved, the quality and qualification rate of the product are improved, and it is suitable for porcelain with high stress and high voltage levels. The billet is fired.
Patent Information
- Application Number
- CN202310614758.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-26
Smart Images

Figure CN116693305B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electric porcelain product production, and in particular relates to a method for firing a porcelain blank to prevent head-turning at a high temperature stage. Background Art
[0002] In the electrical porcelain industry, post insulators are a special type of insulating control component that can play an important role in overhead transmission lines. Most post insulators are solid rod-shaped.
[0003] Solid rod-shaped post insulators have a formed porcelain blank with a burnt head. When the porcelain blank is fired in the kiln, it undergoes a low-temperature drainage stage, a mineral oxidation and decomposition stage, a medium-fire insulation stage, and a reduction stage. During this process, the porcelain blank shrinks in all directions, becomes smaller in size, and gradually hangs on the carbon rod. When designing each rod shape, the burnt stress is not completely consistent. For porcelain blanks with a burnt stress greater than 0.075MPa, at relatively high temperatures, under the influence of the porcelain blank's own weight, the part where the burnt head stress is concentrated will produce rough cracking, and the fallen porcelain will adhere to other porcelain blanks, resulting in a large quality loss.
[0004] It can be seen that the existing firing process method is prone to roughening cracking at the location where the stress of the burnt head is concentrated, and cannot effectively prevent the burnt head of the porcelain blank from falling off, thus affecting the production quality of the product. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preventing the head of a ceramic blank from falling off during firing at a high temperature stage. The method can effectively prevent the ceramic blank from falling off and improve the production quality of the product.
[0006] In order to achieve the above purpose, the present invention adopts the following technical solution:
[0007] A method for firing a ceramic blank to prevent head-turning at a high temperature stage, comprising:
[0008] S1: A main control point is arranged at the bottom of each zone of the kiln, and a secondary control point is arranged at the top;
[0009] S2: In the oxygen permeation preparation transition stage, oxygen permeation start stage and oxygen permeation stable stage, the temperature, pressure, natural gas flow, combustion air flow and ignition valve branch pipe opening in the kiln are controlled respectively, so that the secondary control point temperature in each stage is lower than the main control point temperature, and the porcelain blank is fired.
[0010] Furthermore, in S2, the specific steps of the oxygen permeation preparation transition stage include:
[0011] Control the temperature in the kiln to 1190~1200℃; control the pressure in the kiln to 5.0~5.2Pa; control the natural gas flow in the kiln to 20.5~22.5m 3 / h; control the combustion air flow in the kiln to 220~260m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 22.0~25.0%.
[0012] Furthermore, during the transition stage of oxygen infiltration preparation, the frequency of the smoke exhaust fan is controlled to be 23-25 Hz.
[0013] Furthermore, during the transition stage of oxygen permeation preparation, the temperature of the secondary control point is controlled to be 1 to 3° C. lower than the temperature of the main control point.
[0014] Furthermore, in S2, the specific steps of the initial stage of oxygen permeation include:
[0015] Control the temperature in the kiln to 1200-1210℃; control the pressure in the kiln to 5.2-5.5Pa; control the natural gas flow rate in the kiln to 21.5-22.5m 3 / h; control the combustion air flow in the kiln to 260~300m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 25.0~28.0%.
[0016] Furthermore, during the initial stage of oxygen infiltration, the frequency of the smoke exhaust fan is controlled to be 28 to 30 Hz.
[0017] Furthermore, in the initial stage of oxygen permeation, the temperature of the secondary control point is controlled to be 5 to 8° C. lower than the temperature of the main control point.
[0018] Furthermore, in S2, the specific steps of the oxygen permeation stable stage include:
[0019] Control the temperature in the kiln to 1210℃~fire-stop temperature; control the pressure in the kiln to 5.2~5.5Pa; control the natural gas flow in the kiln to 23.5~26.5m 3 / h; control the combustion air flow in the kiln to 300~360m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 28.0~32.0%.
[0020] Furthermore, during the oxygen permeation stable stage, the frequency of the smoke exhaust fan is controlled to be 33-35 Hz.
[0021] Furthermore, in the oxygen permeation stable stage, the temperature of the secondary control point is controlled to be 8-10°C lower than the temperature of the main control point. Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a method for preventing porcelain blanks from turning around during high-temperature stage firing. The method improves and perfects the firing adjustment method, and is suitable for the firing of rod-shaped products with larger porcelain blanks, especially for the firing of 800kV and higher voltage grade products with larger turning-off stress and higher product quality. The method controls the temperature, pressure, natural gas flow, combustion-supporting air flow and ignition valve branch pipe opening in the kiln in the three stages of oxygen permeation, respectively, and achieves the goal that the upper temperature of each zone is lower than the lower temperature under the premise of ensuring oxygen permeation, thereby effectively preventing the porcelain blanks from turning around during high-temperature stage of high fire, forming a unified standard, and improving the porcelain inspection pass rate of rod-shaped porcelain blank products. The method is simple in principle and operation, easy to implement, and has good promotion value and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of a method for firing a ceramic blank to prevent head turning in a high temperature stage provided by the present invention;
[0024] Figure 2 This is a comparison chart of the water absorption rate of the upper and lower parts of the porcelain bottles in zones 1 to 7 of the first stage and the density of the porcelain body provided by Example 1 of the present invention;
[0025] Figure 3 This is a comparison chart of the water absorption rate of the upper and lower parts of the porcelain bottles in zones 1 to 7 of the second stage and the density of the porcelain body provided by Example 1 of the present invention;
[0026] Figure 4 This is a comparison chart of the water absorption rate and porcelain body density of the upper and lower parts of the porcelain bottles in zones 1 to 7 of the third stage provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] like Figure 1 As shown, the present invention provides a method for firing a ceramic blank to prevent head turning in a high temperature stage, comprising:
[0028] S1: A main control point is arranged at the bottom of each zone of the kiln, and a secondary control point is arranged at the top;
[0029] S2: In the oxygen permeation preparation transition stage, oxygen permeation start stage and oxygen permeation stable stage, the temperature, pressure, natural gas flow, combustion air flow and ignition valve branch pipe opening in the kiln are controlled respectively, so that the secondary control point temperature in each stage is lower than the main control point temperature, and the porcelain blank is fired.
[0030] On the one hand, the specific steps of the oxygenation preparation transition phase include:
[0031] Control the temperature in the kiln to 1190~1200℃; control the pressure in the kiln to 5.0~5.2Pa; control the natural gas flow in the kiln to 20.5~22.5m 3 / h; control the combustion air flow in the kiln to 220~260m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 22.0~25.0%; control the frequency of the smoke exhaust fan to 23~25Hz.
[0032] During the transition stage of oxygen permeation preparation, the temperature of the secondary control point is controlled to be 0 to 3°C lower than the temperature of the main control point.
[0033] On the other hand, the specific steps of the initial stage of oxygenation include:
[0034] Control the temperature in the kiln to 1200-1210℃; control the pressure in the kiln to 5.2-5.5Pa; control the natural gas flow rate in the kiln to 21.5-22.5m 3 / h; control the combustion air flow in the kiln to 260~300m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 25.0~28.0%; control the frequency of the smoke exhaust fan to 28~30Hz.
[0035] In the initial stage of oxygen permeation, the temperature of the secondary control point is controlled to be 5 to 8°C lower than the temperature of the main control point.
[0036] On the other hand, the specific steps of the oxygenation stable stage include:
[0037] Control the temperature in the kiln to 1210℃~fire-stop temperature; control the pressure in the kiln to 5.2~5.5Pa; control the natural gas flow in the kiln to 23.5~26.5m 3 / h; control the combustion air flow in the kiln to 300~360m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 28.0~32.0%; control the frequency of the smoke exhaust fan to 33~35Hz.
[0038] During the oxygen permeation stable stage, the temperature of the secondary control point is controlled to be 8 to 10°C lower than the temperature of the main control point.
[0039] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0040] Example 1
[0041] The present embodiment provides a method for preventing the head of a ceramic blank from falling off during high temperature firing, which can prevent the head of a rod-shaped product from falling off and cracking during high temperature firing (1190°C to the firing temperature). The so-called high temperature refers to the reduction process of firing.
[0042] Here is an example of a kiln (7 zones):
[0043] Each zone has two burners, namely annular tube air inlet burners, and each zone has two control points, which are evenly distributed in 7 zones. Among them, the lower part of each zone is the main control point, and the upper part is the auxiliary control point.
[0044] The first stage, the second stage and the third stage represent the oxygenation preparation transition stage, the oxygenation start stage and the oxygenation stable stage respectively.
[0045] The first stage is (1190~1200)℃. The combustion air flow rate of each zone of the kiln is controlled at (220~260)m 3 / h, natural gas flow rate is controlled at (20.5~22.5)m 3 / h. The pressure in the kiln is controlled at (5.0~5.2)Pa. The opening of the branch pipe of the ignition valve in each zone is adjusted to (22.0~25.0)%, and the frequency of the smoke exhaust fan is (23~25)Hz, so that the actual temperature at the upper part of the point (i.e. the temperature of the auxiliary control point, which will not be repeated below) differs by a maximum of 3℃ from the temperature of the lower main control point. At this time, the kiln is still in the oxygen permeation preparation and transition state, and the ratio of air to gas in each zone is (11.5~13.5):1.
[0046] Specific control examples are as follows:
[0047] Zone 1: Combustion air flow rate is controlled at (220~230)m 3 / h, natural gas flow rate is controlled at (20.5~21.0)m 3 / h, ignition valve branch pipe opening: upper burner adjusted to (22.0 ~ 22.5)%, lower burner adjusted to (22.5 ~ 23.5)%. In this way, the air-fuel ratio of the upper part is slightly larger than that of the lower part, and the reducing atmosphere becomes weaker. At this stage, due to the large flow of combustion-supporting air, the heating speed is relatively slow when the amount of natural gas becomes smaller, thus achieving the goal of lowering the upper temperature by (0 ~ 3) ℃ than the lower temperature.
[0048] Zone 2: Combustion-supporting air flow rate is controlled at (240-250) m 3 / h, natural gas flow rate is controlled at (21.5~22.5)m 3 / h, natural gas ignition valve branch pipe opening: the upper burner opening is adjusted to (23.0~24.0)%, and the lower burner is adjusted to (24~25)%. In this way, the air-fuel ratio of the upper part is also slightly larger than that of the lower part, and the goal of lowering the upper temperature by (0~3)℃ is also achieved.
[0049] Zones 3 to 7 were adjusted according to the ranges and methods mentioned above, as shown in Table 1. In the first stage, the water absorption rate and density of the upper and lower parts of the porcelain bottle were measured respectively:
[0050] Table 1 shows the water absorption rate and density of the upper and lower parts of the porcelain bottles from Zone 1 to Zone 7 in the first stage
[0051] Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 Upper porcelain water absorption 0.48 0.46 0.45 0.45 0.45 0.46 0.47 Water absorption rate of lower porcelain 0.45 0.43 0.42 0.4 0.41 0.42 0.42 Density of upper porcelain 2.72 2.72 2.73 2.73 2.72 2.72 2.72 Density of lower porcelain body 2.74 2.75 2.76 2.76 2.75 2.74 2.74
[0052] Combination Figure 2As shown, it can be seen that since the temperature of the upper part is lower than that of the lower part, the water absorption rate of the upper porcelain is generally lower than that of the lower part, and the corresponding porcelain body density also follows the same rule. In the first stage, the firing temperature did not reach the quenching temperature, the porcelain was not completely sintered, the actual water absorption rate was greater than that of qualified porcelain, and the porcelain body density was greater than that of qualified porcelain. This is a normal phenomenon.
[0053] The second stage is (1200~1210)℃. The combustion air flow rate of each zone of the kiln is controlled at (260~300)m 3 / h, natural gas flow rate is controlled at (21.5~22.5)m 3 / h. The pressure in the kiln is controlled at (5.2~5.5)Pa, and the frequency of the smoke exhaust fan is (28~30)Hz. The opening of the ignition valve branch pipe in each zone is adjusted to (25.0~28.0)%, so that the actual temperature at the top of the point is (5~8)℃ lower than the temperature of the lower main control point. The kiln is still in the initial state of oxygen penetration at this time, and the ratio of air to gas in each zone is (13.5~14.5):1.
[0054] Specific control examples are as follows:
[0055] Zone 1: Combustion air flow rate is controlled at (260~270)m 3 / h, natural gas flow rate is controlled at (21.5~21.8)m 3 / h, natural gas ignition valve branch pipe opening: the upper burner opening is adjusted to (25.0~26)%, and the lower burner is adjusted to (26~27)%. Similarly, the air-fuel ratio of the upper part is slightly larger than that of the lower part, and the reducing atmosphere becomes weaker. At this stage, due to the large flow rate of the combustion-supporting air, the heating speed is relatively slow when the amount of natural gas becomes smaller, which achieves the goal of lowering the upper temperature by (5~8)℃ than the lower temperature.
[0056] Zone 2: Combustion air flow rate is controlled at (270~290)m 3 / h, natural gas flow rate is controlled at (22.0~22.5)m 3 / h, ignition valve branch opening: upper burner adjusted to (26.0~26.5)%, lower burner adjusted to (27.0~28.0)%. At the same time, according to the change of point temperature, each parameter is fine-tuned. In this way, the upper temperature is (5~8)℃ lower than the lower temperature.
[0057] Zones 3 to 7 were adjusted according to the ranges and methods mentioned above, as shown in Table 2. In the second stage, the water absorption rate and density of the upper and lower parts of the porcelain bottle were measured respectively:
[0058] Table 2 shows the water absorption rate and porcelain body density of the upper and lower parts of the porcelain bottles from Zone 1 to Zone 7 in the second stage
[0059] Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 Upper porcelain water absorption 0.18 0.17 0.16 0.16 0.17 0.18 0.18 Water absorption rate of lower porcelain 0.16 0.15 0.14 0.14 0.13 0.13 0.14 Density of upper porcelain 2.73 2.74 2.74 2.74 2.74 2.73 2.73 Density of lower porcelain body 2.76 2.77 2.78 2.78 2.77 2.76 2.75
[0060] Combination Figure 3 As shown, it can be seen that since the temperature of the upper part is lower than that of the lower part, the water absorption rate of the upper porcelain is generally lower than that of the lower part, and the corresponding porcelain body density also follows the same rule. In the second stage, the firing temperature did not reach the quenching temperature, the porcelain was not completely sintered, the actual water absorption rate was greater than that of qualified porcelain, and the porcelain body density was greater than that of qualified porcelain.
[0061] The third stage, (1210℃~fire stopping temperature). The combustion air flow rate of each zone of the kiln is controlled at (300~360)m 3 / h, natural gas flow rate is controlled at (23.5~26.5)m 3 / h. The pressure in the kiln is controlled at (5.2~5.5)Pa, and the frequency of the smoke exhaust fan is (33~35)Hz. The opening of the ignition valve branch pipes in each zone is adjusted to (28.0~32.0)%, so that the actual temperature at the top of the point is (8~10)℃ lower than the temperature of the lower main control point. At this time, the kiln is still in a state of steady increase in oxygen permeation, and the ratio of air to gas is (14.5~16.5):1.
[0062] As the amount of oxygen permeation increases, the weak reducing atmosphere is transformed into a weak oxidizing atmosphere, and the heating speed slows down, which will cause the actual temperature to be lower than the program temperature, and the program needs to be stopped and waited, which will prolong the high temperature time and increase the risk of the porcelain blank turning around. In order to prevent this phenomenon from happening, the flow rate of natural gas in the area will be appropriately increased to ensure that the heating speed is (10-12)℃ / h. By fine-tuning the flow rate of natural gas at each point and the opening of the ignition valve branch pipe, the purpose of achieving different temperatures in the upper and lower parts of the kiln can be achieved.
[0063] Specific control examples are as follows:
[0064] Zone 1: Combustion air flow rate is controlled at (300~310)m 3 / h, natural gas flow rate is controlled at (23.5~24.5)m 3 / h, ignition valve branch pipe opening: upper burner adjusted to (28.0 ~ 29.0)%, lower burner adjusted to (29.0 ~ 30.0)%. In this way, the air-fuel ratio of the upper part is slightly larger than that of the lower part, and the reducing atmosphere becomes weaker. At this stage, due to the large flow of combustion-supporting air, the heating speed is relatively slow when the amount of natural gas becomes smaller. At the same time, according to the change of point temperature, each parameter is fine-tuned. This achieves the goal of lowering the upper temperature by (8 ~ 10) ℃ than the lower temperature.
[0065] Zone 2: Combustion air flow rate is controlled at (320~340)m 3 / h, natural gas flow rate is controlled at (25.0~26.5)m 3 / h, ignition valve branch pipe opening: upper burner adjusted to (29-30)%, lower burner adjusted to (30-31)%. In this way, the air-fuel ratio of the upper part is also slightly larger than that of the lower part. At the same time, according to the change of point temperature, each parameter is fine-tuned. The goal of (8-10)℃ lower temperature of the upper part than that of the lower part is also achieved.
[0066] Zones 3 to 7 were adjusted according to the ranges and methods mentioned above, as shown in Table 2. In the third stage, the water absorption rate and the density of the upper and lower parts of the porcelain bottle were measured respectively:
[0067] Table 3 shows the water absorption rate and porcelain body density of the upper and lower parts of the porcelain bottles from Zone 1 to Zone 7 in the three stages
[0068] Zone 1 Zone 2 Zone 3 Zone 4 Zone 5 Zone 6 District 7 Upper porcelain water absorption 0.05 0.04 0.04 0.04 0.04 0.04 0.05 Water absorption rate of lower porcelain 0.04 0.03 0.03 0.03 0.03 0.03 0.04 Density of upper porcelain 2.76 2.77 2.78 2.78 2.77 2.76 2.75 Density of lower porcelain body 2.78 2.79 2.80 2.80 2.79 2.77 2.77
[0069] Combination Figure 4 As shown, it can be seen that since the temperature of the upper part is lower than that of the lower part, the water absorption rate of the upper part is generally lower than that of the lower part, and the corresponding porcelain body density also follows the same rule. In the third stage, the firing temperature reaches the ignition temperature, the porcelain has been completely sintered, and the actual water absorption rate and porcelain body density of the upper and lower parts reach the standard of qualified porcelain. This method prevents the rod-shaped porcelain from turning around, and at the same time makes the various parameters of the porcelain meet the design requirements.
[0070] The present invention is further explained below by taking a certain partition of a kiln as an example:
[0071] Example 2
[0072] In the first stage, the kiln temperature is heated to 1190℃ and the combustion air flow rate in the kiln is controlled at 220m 3 / h, natural gas flow rate is controlled at 20.5m 3 / h. The pressure in the kiln is controlled at 5.0Pa; the opening of the branch pipe of the ignition valve in each zone is adjusted to 22.0%, and the frequency of the smoke exhaust fan is 23Hz, so that the actual temperature at the upper part of the point is 1°C different from the temperature of the lower main control point.
[0073] In the second stage, the kiln temperature is heated to 1200℃. The combustion air flow rate in the kiln is controlled at 260m 3 / h, the natural gas flow rate is controlled at 21.5m 3 / h. The pressure in the kiln is controlled at 5.2Pa, and the frequency of the smoke exhaust fan is 28Hz. The opening of the ignition valve branch pipe in each zone is adjusted to 25.0%, so that the actual temperature at the top of the point is 5℃ lower than the temperature of the lower main control point.
[0074] In the third stage, the kiln temperature is heated to 1210℃, and the combustion air flow rate in the kiln is controlled at 300m 3 / h, the natural gas flow rate is controlled at 23.5m 3 / h. The pressure in the kiln is controlled at 5.2Pa, and the frequency of the smoke exhaust fan is 33Hz. The opening of the ignition valve branch pipes in each zone is adjusted to 28.0%, so that the actual temperature at the top of the point is 8℃ lower than the temperature of the lower main control point.
[0075] Example 3
[0076] In the first stage, the kiln temperature is heated to 1195℃, and the combustion air flow rate in the kiln is controlled at 240m 3 / h, the natural gas flow rate is controlled at 21.5m 3 / h. The pressure in the kiln is controlled at 5.1Pa; the opening of the branch pipe of the ignition valve in each zone is adjusted to 23%, and the frequency of the smoke exhaust fan is 24Hz, so that the actual temperature at the upper part of the point is 2℃ different from the temperature of the lower main control point.
[0077] In the second stage, the kiln temperature is heated to 1202℃. The combustion air flow rate in the kiln is controlled at 280m 3 / h, natural gas flow rate is controlled at 22m 3 / h. The pressure in the kiln is controlled at 5.3Pa, and the frequency of the smoke exhaust fan is 29Hz. The opening of the ignition valve branch pipes in each zone is adjusted to 26.0%, so that the actual temperature at the top of the point is 6℃ lower than the temperature of the lower main control point.
[0078] In the third stage, the kiln temperature is heated to 1220℃, and the combustion air flow rate in the kiln is controlled at 320m 3 / h, the natural gas flow rate is controlled at 23.5m 3 / h. The pressure in the kiln is controlled at 5.2Pa, and the frequency of the smoke exhaust fan is 33Hz. The opening of the ignition valve branch pipes in each zone is adjusted to 28.0%, so that the actual temperature at the top of the point is 9℃ lower than the temperature of the lower main control point.
[0079] Example 4
[0080] In the first stage, the kiln temperature is heated to 1200℃, and the combustion air flow rate in the kiln is controlled at 260m 3 / h, the natural gas flow rate is controlled at 22.5m 3 / h. The pressure in the kiln is controlled at 5.2Pa; the opening of the branch pipe of the ignition valve in each zone is adjusted to 25.0%, and the frequency of the smoke exhaust fan is changed to 25Hz, so that the actual temperature at the upper part of the point is 3℃ different from the temperature of the lower main control point.
[0081] In the second stage, the kiln temperature is heated to 1210℃. The combustion air flow rate in the kiln is controlled at 300m 3 / h, the natural gas flow rate is controlled at 22.5m 3 / h. The pressure in the kiln is controlled at 5.5Pa, and the frequency of the smoke exhaust fan is 30Hz. The opening of the ignition valve branch pipes in each zone is adjusted to 28.0%, so that the actual temperature at the top of the point is 8℃ lower than the temperature of the lower main control point.
[0082] In the third stage, the kiln temperature is heated to the fire-stopping temperature, and the combustion air flow in the kiln is controlled at 360m 3 / h, the natural gas flow rate is controlled at 26.5m 3 / h. The pressure in the kiln is controlled at 5.5Pa, and the frequency of the smoke exhaust fan is 35Hz. The opening of the ignition valve branch pipes in each zone is adjusted to 32.0%, so that the actual temperature at the top of the point is 10℃ lower than the temperature of the lower main control point.
[0083] The present embodiment provides a method for preventing porcelain blanks from turning around during high-temperature firing, which improves and perfects the firing adjustment method and is suitable for the firing of rod-shaped products with larger porcelain blanks, especially for the firing of 800kV and higher voltage products with greater turning-off stress and higher product quality. By controlling the kiln pressure, combustion-supporting air, temperature-regulating air, flow of natural gas and the opening of the upper and lower parts of the ignition valves in each zone, and the actual temperature of each point, the goal of keeping the upper temperature of each zone lower than the lower temperature is achieved while ensuring oxygen permeability, effectively preventing the porcelain blanks from turning around during high-temperature fire stages, forming a unified standard, and improving the inspection pass rate of rod-shaped porcelain.
[0084] Although the embodiments of the present invention are described above in conjunction with the accompanying drawings and embodiments, the present invention is not limited to the above-mentioned specific embodiments and application fields, and the above-mentioned specific embodiments are only illustrative and instructive, rather than restrictive. Under the guidance of the specification, those skilled in the art can also make many forms without departing from the scope of protection of the claims of the present invention, all of which belong to the scope of protection of the present invention.
Claims
1. A method for firing a ceramic blank to prevent it from turning around during high temperature. It is characterized in that include: S1: A main control point is arranged at the bottom of each zone of the kiln, and a secondary control point is arranged at the top; S2: In the oxygen permeation preparation transition stage, the oxygen permeation start stage and the oxygen permeation stable stage, the temperature, pressure, natural gas flow, combustion air flow and the opening of the ignition valve branch pipe in the kiln are controlled respectively, so that the temperature of the secondary control point in each stage is lower than the temperature of the main control point, and the porcelain blank is fired; The specific steps of the oxygen permeation preparation transition stage include: Control the temperature in the kiln to 1190~1200℃; control the pressure in the kiln to 5.0~5.2Pa; control the natural gas flow in the kiln to 20.5~22.5m 3 / h; control the combustion air flow in the kiln to 220~260m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 22.0~25.0%; The specific steps of the initial stage of oxygen permeation include: Control the temperature in the kiln to 1200-1210℃; control the pressure in the kiln to 5.2-5.5Pa; control the natural gas flow rate in the kiln to 21.5-22.5m 3 / h; control the combustion air flow in the kiln to 260~300m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 25.0~28.0%; The specific steps of the oxygen permeation stable stage include: Control the temperature in the kiln to 1210℃~fire-stop temperature; control the pressure in the kiln to 5.2~5.5Pa; control the natural gas flow in the kiln to 23.5~26.5m 3 / h; control the combustion air flow in the kiln to 300~360m 3 / h; control the opening of the ignition valve branch pipe in the kiln to 28.0~32.0%.
2. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that During the transition stage of oxygen infiltration preparation, the frequency of the smoke exhaust fan is controlled to 23-25Hz.
3. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that During the transition stage of oxygen infiltration preparation, the temperature of the secondary control point is controlled to be 1 to 3°C lower than the temperature of the main control point.
4. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that During the initial stage of oxygen infiltration, the frequency of the smoke exhaust fan is controlled to 28-30 Hz.
5. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that In the initial stage of oxygen permeation, the temperature of the secondary control point is controlled to be 5 to 8°C lower than the temperature of the main control point.
6. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that During the stable oxygen permeation stage, the frequency of the smoke exhaust fan is controlled to 33-35Hz.
7. A method for firing a ceramic blank to prevent head-falling at a high temperature stage according to claim 1, It is characterized in that During the oxygen permeation stable stage, the temperature of the secondary control point is controlled to be 8 to 10°C lower than the temperature of the main control point.
Citation Information
Patent Citations
Firing method capable of completely eradicating high-temperature deformation of dry hollow insulator