Piezoelectric element and method for manufacturing the same

Through the combination of alkaline niobate perovskite oxide and base metal electrode, combined with specific process processing, the problems of high dielectric loss and poor stability of lead-free piezoelectric electromagnetic device compositions are solved, and low-voltage piezoelectric elements are realized. Dielectric loss and high insulation.

CN116710416BActive Publication Date: 2024-10-25NITERRA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280009189.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-29
Filing Date
2022-09-08
Publication Date
2024-10-25
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

The dielectric loss of the existing lead-free piezoelectric electromagnetic device composition is relatively large, which leads to the risk of leakage, dielectric breakdown and temperature increase during high electric field polarization treatment, and it is difficult to obtain stable piezoelectricity when fired in a reducing atmosphere. characteristic.

Method used

A lead-free piezoelectric electromagnetic composition composed of alkali niobate perovskite oxide as the main phase is used, and a base metal is used as the electrode. The piezoelectric composition is manufactured in a reducing atmosphere through pre-baking, molding, electrode formation and co-firing processes. For electrical components, adjust the composition ratio of Ti, Zr, Hf and Ba, Ca, Sr to ensure the solid solution of Mn and these elements, reduce oxygen pores and semiconductorization phenomena, and improve sintering and insulation properties.

Benefits of technology

It effectively reduces dielectric loss, improves insulation, and ensures the stability and durability of piezoelectric elements under high electric fields and high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116710416B_ABST
    Figure CN116710416B_ABST
Patent Text Reader

Abstract

The piezoelectric element comprises: a piezoelectric body formed of a lead-free piezoelectric electromagnetic composition, wherein the lead-free piezoelectric electromagnetic composition comprises a composition formula (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 ) 3+e (wherein the element A1 is at least one of the alkali metals, the element M1 is at least one of Ba, Ca, and Sr, and is 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technology disclosed in this specification relates to a piezoelectric element and a method for manufacturing the piezoelectric element. Background Art

[0002] Conventionally, PZT (lead zirconate titanate) has been widely used as a ceramic exhibiting piezoelectricity. However, since PZT contains lead as a component, the environmental impact has been emphasized, and the development of lead-free piezoelectric ceramics has been required.

[0003] In addition, piezoelectric ceramic electronic components are usually manufactured as follows: a ceramic green sheet that will become a piezoelectric ceramic layer is stacked and co-fired with a conductive film that will become an electrode. As electrode materials, Pt, Ag-Pd alloys, etc. are widely used. However, these electrode materials are relatively expensive and prone to migration. Therefore, in recent years, Ni (nickel), which is cheap and can inhibit migration, has been proposed as a substitute. Ni is easily oxidized when fired in an atmospheric atmosphere, so it needs to be fired in a reducing atmosphere. However, when using lead-containing zirconate titanate-based materials and lead titanate-based materials as piezoelectric ceramic materials, if you want to fire these materials in a reducing atmosphere, the lead will be reduced and the desired stable piezoelectric properties cannot be obtained.

[0004] In recent years, various lead-free piezoelectric ceramic compositions containing alkali niobate perovskite oxides as a main phase have been developed as one of the promising candidates for lead-free piezoelectric ceramic materials that do not contain lead and exhibit piezoelectricity even when fired in a reducing atmosphere (see Patent Documents 1 and 2).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5862983

[0008] Patent Document 2: Japanese Patent No. 6489333 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] The dielectric loss (tan δ) of the lead-free piezoelectric magnet composition is as high as about 5%, which raises concerns about insulation, etc. Therefore, when a polarization treatment with a high electric field at several tens of degrees Celsius is applied or when the device is driven, there are concerns about leakage, dielectric breakdown, or an increased temperature.

[0011] Solutions for solving problems

[0012] The piezoelectric element disclosed in the present specification comprises: a piezoelectric body formed of a lead-free piezoelectric electromagnetic composition, wherein the lead-free piezoelectric electromagnetic composition comprises a composition formula (A1aM1b)c(Nbd1 Mn d2 Ti d3 Zr d4 Hf d5 )O 3+e (wherein, element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, and Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, and e is a value representing oxygen deficiency or excess) the main phase formed by a niobium acid-based perovskite oxide, and satisfying b / (d3 + d4 + d5) ≤ 1; and an electrode, which has a base metal as a main component and is in contact with the piezoelectric body described above.

[0013] In addition, the method for manufacturing a piezoelectric element disclosed in this specification includes the following steps: a pre-baking step of mixing raw materials of a lead-free piezomagnetic composition containing a main phase formed by a niobium acid-based perovskite oxide represented by the compositional formula (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 )O 3+e (wherein, element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, and Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, and e is a value representing oxygen deficiency or excess) and firing to obtain pre-baked powder; a molding step of forming a molded body containing the pre-baked powder; an electrode forming step of forming an electrode layer having a base metal as a main component on the molded body; and a co-firing step of co-firing the molded body and the electrode layer in a reducing atmosphere.

[0014] Effects of the Invention

[0015] According to the piezoelectric element and the method for manufacturing a piezoelectric element disclosed in this specification, dielectric loss can be reduced and insulation can be improved. Description of the Drawings

[0016] Figure 1 It is a cross-sectional view of the piezoelectric element of the embodiment. Detailed Embodiments

[0017] [Summary of the Embodiment]

[0018] (1) The piezoelectric element disclosed in this specification includes: a piezoelectric body formed of a lead-free piezomagnetic composition, the lead-free piezomagnetic composition containing a niobate-based perovskite oxide represented by the compositional formula (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 )O 3+e (wherein element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, and e is a value representing oxygen deficiency or excess), and satisfying b / (d3 + d4 + d5) ≤ 1; and an electrode mainly composed of a base metal and in contact with the piezoelectric body.

[0019] In addition, the manufacturing method of the piezoelectric element disclosed in this specification includes the following steps: a pre-baking step of mixing raw materials of a lead-free piezomagnetic composition containing a niobate-based perovskite oxide represented by the compositional formula (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 )O 3+e (wherein element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, and e is a value representing oxygen deficiency or excess), and satisfying b / (d3 + d4 + d5) ≤ 1, firing to obtain pre-baked powder; a molding step of forming a molded body containing the pre-baked powder; an electrode forming step of forming an electrode layer mainly composed of a base metal on the molded body; and a co-firing step of co-firing the molded body and the electrode layer in a reducing atmosphere.

[0020] According to the above configuration, by making the B site (niobium site) in the niobate-based perovskite oxide contain an appropriate amount of Ti, Zr, and Hf, the sinterability of the piezoelectric body is improved, the dielectric loss is reduced, and the insulation property is improved.

[0021] In addition, it is believed that: Mn is dissolved as an acceptor at the B site, thereby compensating for the charge caused by the oxygen pores formed during reduction sintering, reducing dielectric loss, and improving insulation. However, Mn is not easy to dissolve in niobate-alkali perovskite oxides, and is easily segregated as a different phase in the lead-free piezoelectric magnet composition. On the other hand, when Ba, Ca, and Sr are dissolved in the A site (alkali site), the piezoelectric performance is improved. However, Ba, Ca, and Sr play the role of donors, so there is a concern that the insulation will be reduced due to the semiconductorization of the piezoelectric body.

[0022] It is believed that by adjusting the composition ratio of Ti, Zr, Hf to Ba, Ca, Sr so that b / (d3+d4+d5)≤1, appropriate amounts of Ti, Zr, Hf and Mn are dissolved, and the semiconductorization caused by the solid dissolution of Ba, Ca, Sr in the A site is suppressed, the dielectric loss can be reduced and the insulation properties can be improved.

[0023] 2) In the piezoelectric element according to 1) above, a molar ratio of Mn atoms to Nb atoms (Mn / Nb) contained in the main phase may be 0.003 or more.

[0024] In the method for producing a piezoelectric element according to 1), in the pre-baking step, the molar ratio of Mn atoms to Nb atoms (Mn / Nb) contained in the mixture of the raw materials may be 0.005 or more.

[0025] By adjusting the molar ratio of Mn atoms to Nb atoms as described above, the dielectric loss of the piezoelectric body can be reliably reduced and the insulation property can be improved.

[0026] 3) In the piezoelectric element of 1) above, the average particle size of crystal particles of the alkali niobate perovskite type oxide contained in the main phase may be less than 6 μm.

[0027] If the average grain size of the crystal grains is less than 6 μm, the grain boundary resistance is large, and thus a decrease in the piezoelectric characteristics can be avoided.

[0028] 4) In the piezoelectric element of 1) above, the lead-free piezoelectric magnetic composition may further include a subphase, wherein the subphase has a composition formula A2 1-x Ti 1-x Nb 1+x A compound is formed by a compound represented by the composition formula A3Ti3NbO9 (wherein the element A3 is at least one alkali metal) and a compound represented by the composition formula A5Ti3NbO5 (wherein the element A2 is at least one alkali metal and satisfies 0≤x≤0.15).

[0029] According to this configuration, the piezoelectric characteristics can be improved compared to the case where the lead-free piezoelectric magnet composition has no subphase.

[0030] 5) The piezoelectric element of 1) above may have a structure in which the piezoelectric body and the electrodes are alternately stacked.

[0031] [Details of implementation]

[0032] Specific examples of the technology disclosed in this specification will be described below with reference to the drawings. It should be noted that the present invention is not limited to these examples, and is intended to include all changes within the meaning and scope of the claims and equivalents to the claims.

[0033] <Implementation Method>

[0034] [Piezoelectric element 10]

[0035] The piezoelectric element 10 of the present embodiment includes: a piezoelectric layer 11 (an example of a piezoelectric body), a plurality of internal electrodes 12, 13 (an example of electrodes) in contact with the piezoelectric layer 11, and two external electrodes 14, 15 connected to the internal electrodes 12, 13. The piezoelectric layer 11 is composed of a lead-free piezoelectric magnet composition including a main phase formed of an alkali niobate-based perovskite-type oxide. The internal electrodes 12, 13 have a base metal as a main component, for example, Ni (nickel) as a main component. The piezoelectric layer 11 and the internal electrodes 12, 13 are alternately stacked. More specifically, the piezoelectric layer 11 and the internal electrodes 12, 13 are stacked in the order of piezoelectric layer 11, internal electrode 12, piezoelectric layer 11, internal electrode 13, piezoelectric layer 11..., and one piezoelectric layer 11 is sandwiched by two internal electrodes 12, 13. The two external electrodes 14, 15 are arranged on the outer surface of the stack of the piezoelectric layer 11 and the internal electrodes 12, 13. One end of one of the two internal electrodes 12 and 13 in contact with one piezoelectric layer 11 is connected to an external electrode 14, and one end of the other internal electrode 13 is connected to the other external electrode 15. By applying a voltage between the external electrodes 14 and 15, the piezoelectric layer 11 expands and contracts, and the piezoelectric element 10 as a whole expands and contracts.

[0036] [Constitution of lead-free piezoelectric magnetic composition]

[0037] The lead-free piezoelectric magnetic composition constituting the piezoelectric layer 11 includes a main phase composed of an alkali niobate-based perovskite-type oxide having piezoelectric properties. The alkali niobate-based perovskite-type oxide of the present embodiment is represented by the following composition formula (1).

[0038] (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 ) 3+e …(1)

[0039] Element A1 is at least one of alkali metals. Element M1 is at least one of Ca (calcium), Sr (strontium), and Ba (barium) belonging to alkaline earth metals.

[0040] In the above compositional formula (1), element A1 and element M1 are arranged at the A site (alkali site) of the perovskite structure, and Nb (niobium), Mn (manganese), Ti (titanium), Zr (zirconium), and Hf (hafnium) are arranged at the B site.

[0041] As the values of coefficients a to e in the above compositional formula (1), among the combinations of values that enable the perovskite structure to hold, values are selected that are preferable from the viewpoints of the electrical properties or piezoelectric properties (especially the piezoelectric constant d33) of the lead-free piezomagnetic composition.

[0042] Specifically, coefficients a and b satisfy 0 < a < 1, 0 < b < 1, and a + b = 1, excluding a = 0 (i.e., a composition containing no arbitrary alkali metal) and b = 0 (i.e., a composition containing neither Ca, Sr, nor Ba).

[0043] Coefficient c with respect to the entire A site satisfies 0.80 < c < 1.10, preferably 0.84 ≤ c ≤ 1.08, and more preferably 0.88 ≤ c ≤ 1.07.

[0044] Coefficients d1, d2, d3, d4, and d5 satisfy 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, and d1 + d2 + d3 + d4 + d5 = 1. Excluding d1 = 0 (a composition containing no Nb), d2 = 0 (a composition containing no Mn), and d3 = 0 (a composition containing no Ti). The coefficient d4 of Zr and the coefficient d5 of Hf can be zero (i.e., the composition contains neither one or both of Zr or Hf).

[0045] In the coefficient 3 + e of oxygen, coefficient e is a positive or negative value representing oxygen deficiency or excess with respect to the coefficient of oxygen, which is usually 3. The coefficient (3 + e) of oxygen can take a value that forms a perovskite-type oxide as the main phase. A typical value of coefficient e is e = 0, preferably 0 ≤ e ≤ 0.1. It should be noted that the value of coefficient e can be calculated from the electrical neutrality condition of the composition of the main phase. Among them, as the composition of the main phase, a composition slightly deviated from the electrical neutrality condition is also allowed.

[0046] Coefficients b, d3, d4, and d5 satisfy b / (d3 + d4 + d5) ≤ 1. If coefficients b, d3, d4, and d5 take values within this range, a lead-free piezomagnetic composition with low dielectric loss and high insulation can be obtained. The reason is speculated as follows.

[0047] By making the B-site (niobium site) in the niobate-based perovskite oxide contain an appropriate amount of Ti, Zr, and Hf, the sinterability of the piezoelectric body is improved, the dielectric loss is reduced, and the insulation property is improved.

[0048] In addition, it is considered that Mn is dissolved in the B-site as an acceptor, thereby compensating for the charge caused by the oxygen pores formed during reduction firing, reducing the dielectric loss, and improving the insulation property. However, Mn is not easily dissolved in the niobate-based perovskite oxide and is likely to segregate as a heterogeneous phase in the lead-free piezoelectric composition. On the other hand, if Ba, Ca, Sr are dissolved in the A-site (alkali site), the piezoelectric properties are improved. However, since Ba, Ca, Sr act as donors, there is a concern that the insulation property may be reduced due to the semiconductorization of the piezoelectric body.

[0049] It is considered that by adjusting the composition ratio of Ti, Zr, Hf and Ba, Ca, Sr so that b / (d3 + d4 + d5) ≤ 1, an appropriate amount of Ti, Zr, Hf and Mn are dissolved, and the semiconductorization caused by the dissolution of Ba, Ca, Sr in the A-site is suppressed, the dielectric loss can be reduced, and the insulation property can be improved.

[0050] The niobate-based perovskite oxide represented by the above compositional formula (1) preferably contains at least one of K (potassium), Na (sodium), and Li (lithium) as element A1. When the above oxide contains at least one of K, Na, Li as element A1 and contains at least one of Ca, Sr, Ba as element M1, the compositional formula (1) can be rewritten as the following compositional formula (1a).

[0051] (K a1 Na a2 Li a3 Ca b1 Sr b2 Ba b3 ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 )O 3+e …(1a)

[0052] The above compositional formulas (1) and (1a) are equivalent, with a1 + a2 + a3 = a and b1 + b2 + b3 = b. The coefficients a1 and a2 of K and Na are typically 0 < a1 ≤ 0.6 and 0 < a2 ≤ 0.6. The coefficient a3 of Li can be zero, but preferably 0 < a3 ≤ 0.2, and more preferably 0 < a3 ≤ 0.1.

[0053] Among the niobate-alkali perovskite-type oxides represented by the above composition formula (1a), the oxides containing K, Na, and Nb as the main metal components are called "KNN" or "KNN materials". By using this oxide, a lead-free piezoelectric and electromagnetic composition having excellent piezoelectric properties, electrical properties, insulation properties, and high-temperature durability, and having no drastic changes in properties between -50°C and +150°C, can be obtained. The typical composition of the main phase is (K, Na, Li, Ca, Ba) c (Nb, Mn, Ti, Zr, Hf)O 3+e .

[0054] The lead-free piezoelectric magnet composition of the present embodiment may include a subphase formed of an oxide represented by the following composition formula (2) or an oxide represented by the following composition formula (3).

[0055] A2 1-x Ti 1-x Nb 1+x O5…(2)

[0056] A3Ti3NbO9…(3)

[0057] In the composition formula (2), the element A2 is at least one of the alkali metals, preferably at least one of K, Rb (rubidium), and Cs (cesium). The coefficient x satisfies 0≤x≤0.15. If the coefficient x takes a value in this range, the structure of the subphase is stable and a uniform crystalline phase can be obtained. From the viewpoint of the structural stability of the subphase, for the coefficient x, when the element A2 is K or Rb, it is preferably satisfied 0≤x≤0.15, and when the element A2 is Cs, it is preferably satisfied 0≤x≤0.10.

[0058] In the composition formula (3), the element A3 is at least one kind of alkali metals, preferably at least one kind of K, Rb, and Cs.

[0059] The secondary phase does not have piezoelectric properties, but it is believed that the presence of the secondary phase mixed with the primary phase improves sintering properties and also improves insulation properties. In addition, it is also beneficial for operations such as not generating a phase transition point between -50°C and +150°C. The secondary phase is a layered compound (or layered compound), and when it is a layered compound, it is presumed to be beneficial for improving the insulation properties of the piezoelectric magnet composition and not generating a phase transition point.

[0060] The content ratio of the subphase may be more than 0 mol % and less than 20 mol %, preferably 2 mol % or more and 15 mol % or less, and more preferably 2 mol % or more and 10 mol % or less.

[0061] Among the oxides represented by composition formula (2) or (3), oxides containing Nb, Ti and K as main metal components are referred to as “NTK materials.” By using such oxides, it is possible to obtain a lead-free piezoelectric magnetic composition that is inexpensive and has excellent piezoelectric properties.

[0062] The molar ratio of Mn atoms to Nb atoms (Mn / Nb) contained in the main phase is preferably 0.003 or more. By adjusting in this way, the dielectric loss of the piezoelectric layer 11 can be reliably reduced, and the insulation property can be improved.

[0063] The average particle size of the crystal particles of the alkali niobate perovskite oxide contained in the main phase is preferably less than 6 μm. If the average particle size of the crystal particles is less than 6 μm, the grain boundary resistance is large, and thus a decrease in piezoelectric characteristics can be avoided.

[0064] [Method of Manufacturing Piezoelectric Element 10]

[0065] An example of a method for manufacturing the piezoelectric element 10 is described below.

[0066] 1. Pre-calcination process

[0067] First, select the desired ones from the raw material powders of the main phase and weigh them in a manner to achieve the target composition. The raw material powders can be oxides, carbonates, and hydroxides of the elements contained in the main phase. At this time, the molar ratio of Mn atoms to Nb atoms (Mn / Nb) contained in the mixture of the raw material powders of the main phase is made to be 0.005 or more. Ethanol is added to these raw material powders, and wet mixing is preferably performed in a ball mill for more than 15 hours to obtain a slurry. The obtained slurry is dried to obtain a mixed powder, and the obtained mixed powder is pre-baked at 600 to 1000° C. for 1 to 10 hours, for example, under an atmospheric atmosphere to obtain a pre-baked product of the main phase (pre-baking process).

[0068] The upper limit of the molar ratio (Mn / Nb) of Mn atoms to Nb atoms contained in the mixture of the raw material powders of the main phase is not particularly limited, but Mn / Nb ≤ 0.1 is preferred. If the molar ratio (Mn / Nb) is greater than 0.1, sintering may become difficult.

[0069] In addition, the desired raw material powders are selected from the raw material powders of the secondary phase and weighed in a manner to obtain the target composition. The raw material powders may be oxides, carbonates, or hydroxides of the elements contained in the secondary phase. Then, ethanol is added to these raw material powders, and wet mixing is preferably performed in a ball mill for more than 15 hours to obtain a slurry. The obtained slurry is dried to obtain a mixed powder, and the obtained mixed powder is pre-baked at 600 to 1000° C. for 1 to 10 hours in, for example, an atmospheric atmosphere to obtain a secondary phase pre-baked product.

[0070] Next, the pre-baked main phase and the pre-baked sub-phase are weighed, and a dispersant, a binder, and an organic solvent such as toluene are added and pulverized / mixed to form a slurry. Thereafter, the slurry is processed into a sheet shape using a doctor blade method or the like to form a ceramic green sheet (an example of a molded body) (molding step).

[0071] Next, an electrode layer to be an internal electrode is formed on one side of the ceramic green sheet using a conductive paste for internal electrodes, for example, by screen printing (electrode forming step). The electrode layer contains a base metal as a main component, for example, Ni as a main component.

[0072] Next, a plurality of ceramic green sheets with electrode layers are stacked, and ceramic green sheets without electrode layers are further stacked on the front and back sides thereof and pressed together to obtain a laminated body in which ceramic green sheets and electrode layers are alternately stacked. The laminated body is cut into a desired shape and then maintained at 200 to 400° C. for 2 to 10 hours, for example, to perform a binder removal treatment.

[0073] The laminated body after the binder removal treatment is sintered at 900 to 1200° C. for 2 to 5 hours in a reducing atmosphere adjusted to an oxygen partial pressure that does not oxidize the electrode layer (co-sintering step).

[0074] For example, an external electrode made of Au is formed on the outer surface of the fired laminate by sputtering, and polarization treatment is performed to obtain a piezoelectric element.

[0075] It should be noted that the above manufacturing method is an example, and various other processes and processing conditions for manufacturing piezoelectric elements can be used. For example, the raw materials can be mixed and fired in a quantitative ratio that meets the composition of the final lead-free piezoelectric magnet composition instead of pre-baking the main phase and the auxiliary phase separately, and then the powders of the two are mixed and fired. Among them, according to the method of mixing the pre-baked products of the main phase and the auxiliary phase separately in advance, it is easy to more strictly manage the composition of the main phase and the auxiliary phase, so the yield of the lead-free piezoelectric magnet composition can be improved.

[0076] The lead-free piezoelectric magnet composition and piezoelectric element of this embodiment can be widely used for vibration detection purposes, pressure detection purposes, oscillation purposes and piezoelectric device purposes, etc. For example, it can be used for sensors for detecting various vibrations (knock-in sensors and combustion pressure sensors, etc.), piezoelectric devices such as vibrators, actuators, filters, high voltage generating devices, micro power supplies, various driving devices, position control devices, vibration suppression devices, fluid discharge devices (paint discharge and fuel discharge, etc.), etc. In addition, the lead-free piezoelectric magnet composition and piezoelectric element of this embodiment are particularly suitable for applications requiring excellent thermal durability (such as knock-in sensors and combustion pressure sensors, etc.).

[0077] It should be noted that, in this embodiment, an example is shown in which the piezoelectric element 10 has a structure in which the piezoelectric layer 11 and the internal electrodes 12 and 13 are alternately stacked, but the piezoelectric element can also be a piezoelectric element with a single-layer structure having a piezoelectric body and an electrode arranged on the surface of the piezoelectric body.

[0078] <Test example>

[0079] 1. Test Example 1

[0080] (1) Preparation of samples

[0081] K2CO3 powder, Na2CO3 powder, and Nb2O5 powder were weighed and mixed so that the coefficients f and g of the following composition formula (2) would have the ratios shown in Table 1.

[0082] (K f Na g )NbO3…(2)

[0083] In addition, a desired one is selected from BaCO3 powder, CaCO3 powder, and SrCO3 powder, and is weighed and added in such a manner that the total molar percentage of Ba atoms, Ca atoms, and Sr atoms relative to Nb atoms contained in Nb2O5 powder becomes the value shown in Table 1. In addition, MnO2 powder, TiO2 powder, ZrO2 powder, and HfO2 powder are weighed and added in such a manner that the molar percentage of metal atoms in the powder relative to Nb atoms contained in Nb2O5 powder becomes the value shown in Table 1.

[0084] Ethanol is added to the mixture of these raw material powders, and wet mixing is performed in a ball mill for more than 15 hours to obtain a slurry. The obtained slurry is dried to obtain a mixed powder, and the obtained mixed powder is pre-baked at 600°C to 1000°C for 1 to 10 hours in an air atmosphere to obtain a pre-baked powder.

[0085] The obtained pre-baked powder is added with a dispersant, a binder, and an organic solvent such as toluene, and then crushed / mixed to form a slurry. Thereafter, the slurry is processed into a sheet shape using a doctor blade method to form a ceramic green sheet. After stacking a plurality of obtained ceramic green sheets and pressing them together, they are cut into a disk shape to obtain a molded body.

[0086] By screen printing, a conductive paste for electrode is applied to both sides of the obtained molded body to form an electrode layer (electrode forming process). The content ratio of the electrode components contained in the conductive paste for electrode is shown in Table 2. For sample No. 1-24, Ni is set to 100%, and for sample No. 25, Cu is set to 90 mass% and Ni is set to 10 mass%.

[0087] The molded body with the electrode layer formed thereon is kept at 200-400°C for 2-10 hours, subjected to a binder removal treatment, and then kept at 900-1200°C for 2-5 hours in a reducing atmosphere with an oxygen partial pressure controlled so that the electrode layer is not oxidized, and co-fired. The obtained sintered body is subjected to a polarization treatment by applying an electrolysis of 5 kV / mm in silicone oil at 50°C, and is used as a sample. The obtained sample is a piezoelectric body composed of a lead-free piezoelectric electromagnetic composition formed of an alkali niobate perovskite-type oxide represented by the above composition formula (1a), and a piezoelectric element having an electrode layer formed on the surface of the piezoelectric body.

[0088] [Table 1]

[0089]

[0090] (2) Test methods

[0091] The obtained samples were measured using an impedance analyzer (Keysight Technologies, E4990A), and the dielectric loss tanδ was calculated from the value of the electrostatic capacitance at room temperature and 1kHz. In addition, the electromechanical coupling coefficient kp was obtained by the resonance-antiresonance method. The samples with a dielectric loss tanδ of 3.0% or less and an electromechanical coupling coefficient kp of 20% or more were judged to be excellent.

[0092] In addition, the obtained samples were subjected to a dielectric breakdown test. Specifically, in silicone oil at 50°C, 5 kV / mm electrolysis was applied for more than 30 minutes to investigate whether dielectric breakdown occurred. The case where dielectric breakdown occurred was evaluated as ×, and the case where dielectric breakdown did not occur was evaluated as 0.

[0093] (3) Results

[0094] For each sample, the total molar percentage of Ca atoms, Sr atoms, and Ba atoms relative to Nb atoms in the mixture of raw material powders weighed in 1. (1) above is referred to as P. M1 The molar percentages of Ti atoms, Zr atoms, and Hf atoms relative to Nb atoms are denoted by P, Ti , P Zr , P Hf , find P M1 / (P Ti +P Zr +P Hf ) value. In addition, for each sample, an electron probe microanalyzer (EPMA) was used to analyze the beam diameter of Under the condition of 3 points, elemental analysis was performed on the particles of the main phase to measure the molar ratio of Mn atoms to Nb atoms, and the average value of the three points was calculated as the molar ratio of Mn atoms to Nb atoms contained in the main phase (Mn / Nb). These values ​​are shown in Table 2 together with the results of the dielectric loss tanδ, electromechanical coupling coefficient kp, and dielectric breakdown test.

[0095] [Table 2]

[0096]

[0097] Here, theoretically, all of the Ca atoms, Sr atoms, and Ba atoms in the raw material powder enter the A site of the obtained niobate-alkali perovskite oxide. In addition, all of the Ti atoms, Zr atoms, and Hf atoms enter the B site of the obtained niobate-alkali perovskite oxide. Therefore, it can be considered that the total molar percentage PM1 of Ba atoms, Ca atoms, and Sr atoms corresponds to the total value of the coefficients b1, b2, and b3 of Ba, Ca, and Sr in the above composition formula (1a) (the value of the coefficient b in the composition formula (1)), and it can be considered that the molar percentages of Ti atoms, Zr atoms, and Hf atoms correspond to the coefficients d3, d4, and d5 of Ti, Zr, and Hf in the above composition formula (1), respectively. From the above, it can be considered that the relationship between the molar percentages P M1 / (P Ti +P Zr +P Hf ) is equivalent to the relationship b / (d3+d4+d5) among the coefficients b, d2, and d3 in the composition formula (1).

[0098] P M1 / (P Ti +P Zr +P Hf ) value (i.e., the value of b / (d3+d4+d5)) of 1 or more, the dielectric loss of samples No. 1 and 2 was more than 3.0%, and dielectric breakdown occurred in the dielectric breakdown test. The dielectric loss of sample No. 3 not containing Mn was also more than 3.0%, and dielectric breakdown occurred in the dielectric breakdown test. The dielectric loss of sample No. 4 not containing Ti was also more than 3.0%, and dielectric breakdown occurred in the dielectric breakdown test. Furthermore, sample No. 10, in which the molar percentage of Mn atoms contained in the mixture of raw materials to Nb atoms was 0.1% (i.e., the molar ratio of Mn atoms contained in the mixture of raw materials to Nb atoms (Mn / Nb) was 0.001), also had a dielectric loss of more than 3.0%, and dielectric breakdown occurred in the dielectric breakdown test.

[0099] Sample No. 5-9 and Sample No. 11-25 contain element A1 (at least one of alkali metals), element M1 (at least one of Ba, Ca, Sr), Mn and Ti as essential components, P M1 / (P Ti +P Zr +P Hf ) value (i.e., the value of b / (d3+d4+d5)) is 1 or less, the molar percentage of Mn atoms contained in the raw material mixture relative to Nb atoms is 0.5% or more (i.e., the molar ratio of Mn atoms contained in the raw material mixture relative to Nb atoms (Mn / Nb) is 0.005 or more), and the molar ratio of Mn atoms contained in the main phase relative to Nb atoms (Mn / Nb) is 0.003 or more. The dielectric loss of these samples is 3.0% or less, the electromechanical coupling coefficient is 20% or more, and no dielectric breakdown occurs in the dielectric breakdown test, confirming that the piezoelectric properties are excellent.

[0100] 2. Test Example 2

[0101] (1) Preparation of samples and test methods

[0102] Samples No. 26 to 29 (see Table 3) having the same composition as Sample No. 5 were obtained in the same manner as in Test Example 1. These samples were adjusted so that the particle sizes of the crystal particles of the alkali niobate perovskite oxide were different from each other by varying the sintering temperatures in the sintering step.

[0103] [Table 3]

[0104]

[0105] The sample was photographed at 5000 times with SEM (manufactured by Hitachi High-Tech Corporation, TM4000Plus), and the average value of the particle size of the crystal particles contained in the obtained image was taken as the average particle size. In addition, for the obtained sample, the dielectric loss tanδ and the electromechanical coupling coefficient kp were obtained in the same manner as in the above-mentioned Test Example 1, and a dielectric breakdown test was performed.

[0106] (2) Results

[0107] For each sample, the dielectric loss tan δ, the electromechanical coupling coefficient kp, and the results of the dielectric breakdown test are shown in Table 4 together with the average particle size.

[0108] [Table 4]

[0109]

[0110] The dielectric loss of sample No. 29, which contained crystal particles with an average particle size of 6 μm, was 3.0% or more, and dielectric breakdown occurred in the dielectric breakdown test. In contrast, the dielectric loss of sample No. 5, which contained crystal particles with an average particle size of less than 6 μm, and samples No. 26-28 were 3.0% or less, and the electromechanical coupling coefficient was 20% or more. No dielectric breakdown occurred in the dielectric breakdown test, confirming excellent piezoelectric properties.

[0111] Description of Reference Numerals

[0112] 10: Piezoelectric element

[0113] 11: Piezoelectric layer (piezoelectric body)

[0114] 12, 13: Internal electrode (electrode)

Claims

1. A piezoelectric element, comprising: A piezoelectric body, wherein the piezoelectric body is formed of a lead-free piezoelectric electromagnetic composition, wherein the lead-free piezoelectric electromagnetic composition comprises a composition formula (A1 a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 ) 3+e The main phase is formed by the niobate-alkali perovskite oxide shown in the figure. Wherein, Element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, e is a value representing oxygen deficiency or excess, and satisfies b / (d3 + d4 + d5) ≤ 1; And, An electrode, which uses a base metal as a main component and is in contact with the piezoelectric body, Wherein, the molar ratio Mn / Nb of Mn atoms contained in the main phase to Nb atoms is 0.003 or more, The average particle diameter of the crystal grains of the niobium acid-base system perovskite-type oxide contained in the main phase is less than 6 μm.

2. The piezoelectric element according to claim 1, Wherein, The lead-free piezoelectric magnetic composition further comprises a subphase, wherein the subphase has a composition formula A2 1-x Ti 1-x Nb 1+x O 5 The compound shown, and the composition formula A3Ti 3 NbO 9 A compound of one of the compounds shown is formed, wherein the element A2 is at least one of alkali metals, 0≤x≤0.15 is satisfied, and the element A3 is at least one of alkali metals.

3. The piezoelectric element according to claim 1 or 2, which has a structure in which the piezoelectric body and the electrode are alternately laminated.

4. A method for manufacturing a piezoelectric element, comprising the following steps: In the pre-baking step, the a M1 b ) c (Nb d1 Mn d2 Ti d3 Zr d4 Hf d5 ) 3+e The raw materials of the lead-free piezoelectric magnetic composition having a main phase formed of an alkali niobate-based perovskite-type oxide and satisfying b / (d3+d4+d5)≤1 are mixed and fired to obtain a pre-baked powder, Wherein, Element A1 is at least one of alkali metals, element M1 is at least one of Ba, Ca, Sr, 0 < a < 1, 0 < b < 1, a + b = 1, c satisfies 0.80 < c < 1.10, 0 < d1 < 1, 0 < d2 < 1, 0 < d3 < 1, 0 ≤ d4 < 1, 0 ≤ d5 < 1, d1 + d2 + d3 + d4 + d5 = 1, e is a value representing oxygen deficiency or excess; A molding step of forming a molded body containing the pre-baked powder; An electrode forming step of forming an electrode layer using a base metal as a main component on the molded body; and, A co-firing step of co-firing the molded body and the electrode layer in a reducing atmosphere, Wherein, the average particle diameter of the crystal grains of the niobium acid-base system perovskite-type oxide contained in the main phase is less than 6 μm, In the pre-baking step, the molar ratio Mn / Nb of Mn atoms contained in the mixture of the raw materials to Nb atoms is 0.005 or more.

Citation Information

Patent Citations

  • Piezoelectric element, piezoelectric device and method of manufacturing piezoelectric element

    CN103579491A

  • Lead-free piezo-electric porcelain composition, piezo-electric element using the same, and method for producing lead-free piezo-electric porcelain composition

    CN104973863A

  • Piezoelectric ceramic and method of producing the same

    JP2005179144A

  • Piezoelectric ceramic, piezoelectric element and method of producing piezoelectric ceramic

    JP2014177355A

  • Oxide body, piezoelectric device, and liquid discharge device

    US20080302658A1