A method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation
By forming a dense nanocarbon black layer on the surface of graphite particles and using phenolic resin impregnation and high-temperature carbonization, the problem of insufficient carbon content of silicified graphite materials in the existing technology is solved, the preparation of high carbon content silicified graphite is achieved, the process is simplified and the process is improved. material properties.
Patent Information
- Application Number
- CN202310698196.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-06-13
AI Technical Summary
It is difficult to prepare siliconized graphite material with high carbon content through reactive infiltration method in the existing technology, resulting in failure to fully exert its self-lubricating properties, complicated process and high cost.
By forming a dense nanocarbon black layer on the surface of graphite particles, using phenolic resin impregnation and high-temperature carbonization, and then performing reaction infiltration and sintering under vacuum and high temperature, a high carbon content silicided graphite material is formed.
The high carbon phase content of the silicified graphite material is achieved, its self-lubricating performance is improved, the process flow is simplified, and the cost is reduced. The density and compactness reach 2.6~2.8g·cm-3, and the open porosity is less than 1%.
Smart Images

Figure CN116715524B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of inorganic non-metallic materials, and particularly relates to a preparation method of high-carbon silicified graphite based on nano carbon black and resin impregnation. Background Art
[0002] Silicified graphite material is a composite material composed of carbon, silicon carbide and silicon after graphite is silicified. It combines the advantages of graphite and silicon carbide materials. It not only has good self-lubricating properties, low thermal expansion coefficient, excellent high temperature strength and good thermal shock resistance, but also has a series of characteristics such as high strength, high hardness, oxidation resistance and corrosion resistance. It is an ideal structural material. Therefore, silicified graphite materials are widely used in bearing bushes, thermal structural materials, thermocouple protection tubes and other fields. They are suitable for mechanical seal friction pairs and thrust bearing bushes used in shielded pumps, centrifugal pumps and compressors in harsh environments. At present, the main methods for preparing silicified graphite composite materials are: chemical vapor infiltration, chemical vapor reaction, precursor impregnation cracking and reactive melt infiltration. Compared with the first three methods, the reactive melt infiltration method for preparing silicified graphite ceramics has the advantages of simple molding, low cost, low sintering temperature, one-time sintering density, fast sintering speed and near net size. At high temperatures, the silicon-carbon contact angle is very small and the reaction is very violent, which causes the carbon source in the ordinary porous body to easily react with liquid silicon to form silicon carbide, resulting in a low carbon content in the silicified graphite material. Therefore, how to prepare silicified graphite materials with high carbon content by reactive infiltration and make them exert excellent self-lubricating properties is the key preparation technology.
[0003] The Chinese invention patent (Method for preparing silicified graphite by carbon source modification and reactive infiltration and silicified graphite, 202111249322.6) prepares silicified graphite material by mixing graphite particles with resin, solidifying, carbonizing, and crushing to obtain composite particles, and then reactive infiltration. This method requires the preparation of composite particles first, and the process has many steps and is relatively complicated. Moreover, after obtaining the composite particles, they need to be crushed and pre-pressed by a hydraulic press before cold isostatic pressing, and the process flow is complicated.
[0004] In the Chinese invention patent (graphite modification method and modified graphite obtained, 200610119250.2), graphite and high molecular polymer are fully mixed, and heated and cured in stages to obtain a graphite material with a surface coated with high molecular polymer. However, in this invention patent, the high molecular polymer is coated on the graphite surface to solve the problem of graphite layer peeling and pulverization caused by the co-insertion of lithium ions and electrolyte, thereby reducing the capacity attenuation caused thereby and extending the cycle life of the electrode, and it is not to obtain a silicified graphite material with a high carbon content.
[0005] The Chinese invention patent (A method for preparing C / SiC composite materials by low-cost molten silicon infiltration, 201310290077.2) mentions using phenolic resin to impregnate the sintered body after primary siliconization, and then performing secondary siliconization after carbonization. However, the role of the phenolic resin is to react with silicon as a carbon source to generate silicon carbide after carbonization, so as to improve the density of the carbon / silicon carbide material and reduce the pore content and free silicon content. Therefore, silicified graphite with a high carbon content cannot be obtained.
[0006] Therefore, how to provide a method for preparing silicified graphite with high carbon content is a technical problem that urgently needs to be solved. Summary of the invention
[0007] In order to solve the above-mentioned defects existing in the prior art, the purpose of the present invention is to provide a method for preparing high-carbon silicified graphite based on nano-carbon black and resin impregnation, by forming a dense nano-carbon black layer on the surface of graphite particles, which preferentially reacts with silicon in the reactive infiltration to form a dense, thinner silicon carbide layer to prevent further reaction of carbon and silicon, effectively protecting the coated graphite particles, thereby realizing the preparation of silicified graphite with a high carbon content.
[0008] The present invention is achieved through the following technical solutions.
[0009] According to one aspect of the present invention, there is provided a method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation, comprising the following steps:
[0010] (1) mechanically mixing spherical graphite and nano carbon black, and pressing the uniformly mixed powder into a shape to obtain a green body;
[0011] (2) immersing the green body in phenolic resin under pressure, cleaning the surface and drying it;
[0012] (3) subjecting the impregnated and dried green body to high-temperature carbonization under a protective atmosphere to obtain porous carbon;
[0013] (4) placing the porous carbon on a crucible with silicon particles on the bottom, adding another layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, and performing reaction infiltration, sintering, heat preservation, and cooling under vacuum and high temperature to obtain silicified graphite material.
[0014] As a preferred solution, spherical graphite and nano carbon black are mechanically mixed in a mass ratio of 80-95%:5-20%.
[0015] As a preferred solution, the pressure of powder pressing is 30-40 MPa, and the holding time is 20-40 s.
[0016] As a preferred solution, the green body is immersed in the phenolic resin under pressure of 0.6-0.8 MPa and the pressure holding time is 2-6 hours.
[0017] As a preferred solution, the protective atmosphere is nitrogen or argon.
[0018] As a preferred solution, the heating rate during carbonization is 1°C / min, the carbonization temperature is 800-1200°C, and the holding time is 2-4h.
[0019] As a preferred solution, the reaction infiltration sintering temperature is 1450-1650°C, and the holding time is 10-60 minutes.
[0020] As a preferred solution, the vacuum degree of reactive infiltration is 10 Pa or less.
[0021] According to another aspect of the present invention, there is provided a high carbon silicified graphite prepared by the method based on nano carbon black and resin impregnation.
[0022] The present invention adopts the above technical solution, which has the following beneficial effects:
[0023] By controlling the mechanical mixing ratio of nano carbon black particles and spherical graphite, as well as the pressure of powder pressing, a dense nano carbon black coating layer with high purity, small particle size and large specific surface area is formed on the surface of graphite particles; the formed green body is impregnated in resin, and the resin can be well bonded under high pressure, and the green body becomes very dense after high-temperature carbonization. The dense nano carbon black layer on the surface of graphite particles preferentially reacts with silicon in the reaction infiltration to form a dense and thinner silicon carbide layer to prevent further reaction of carbon and silicon, effectively protect the coated graphite particles, increase the content of carbon phase in silicified graphite, and thus improve the self-lubricating properties of the material.
[0024] The silicified graphite composite material prepared by the preparation method has a carbon content of 39.25 vol.%, and a density of 2.6-2.8 g·cm -3 , open porosity is less than 1%.
[0025] In addition, the silicified graphite material prepared by the present invention is dense, has a high carbon phase content, and has a simple preparation process, low energy consumption, and a short production cycle. It has broad application prospects in the fields of chemical industry, metallurgy, environmental protection, national defense, aerospace, nuclear energy, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0027] Figure 1is a SEM image of silicified graphite prepared in Example 3 of the present invention;
[0028] Figure 2 It is a SEM picture of the silicified graphite prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0030] The present invention provides a method for preparing high-carbon silicified graphite based on nano-carbon black and resin impregnation, comprising:
[0031] Step 1, mechanically mix spherical graphite and nano carbon black in a mass ratio of 80-95%:5-20%, put the evenly mixed powder into a mold, and use a hydraulic press to press and form, the pressing pressure is 30-40MPa, and the holding time is 20-40s.
[0032] In step 1, due to the high purity and small particle size of nano carbon black, after mechanical mixing, the nano carbon black is uniformly adsorbed on the surface of spherical graphite to form a continuous and relatively dense nano carbon black layer. The nano carbon black layer will preferentially react with silicon during the reaction infiltration process, effectively protecting the coated graphite particles. By further optimizing the ratio of spherical graphite to nano carbon black, the adhesion effect of nano carbon black on the surface of spherical graphite is improved, and the protection effect is improved.
[0033] In step 1, a green body with a certain strength and porosity can be made by compression molding at a certain pressure, ensuring the smooth progress of reactive infiltration. By optimizing the compression molding pressure and holding time, a better infiltration effect can be achieved to ensure the successful infiltration of liquid silicon.
[0034] Step 2, using phenolic resin as an impregnating agent, placing the green body in an autoclave at a temperature of 25 to 35° C., pressurizing it to 0.6 to 0.8 MPa, using negative pressure to absorb the phenolic resin into it, maintaining the pressure and impregnating it for 2 to 6 hours, then releasing the pressure to take out the green body, cleaning the surface and drying it, to obtain the green body after impregnation and drying;
[0035] Step 3, placing the impregnated and dried green body in a tubular furnace under a protective atmosphere of nitrogen or argon for carbonization, the heating rate during carbonization is 1°C / min, the carbonization temperature is 800-1200°C, and the holding time is 2-4h to obtain porous carbon;
[0036] In steps 2 and 3, phenolic resin is used as an impregnating agent. The resin can be well bonded to the particles under high pressure, and the green body can become very dense after high-temperature carbonization. The resin impregnation can be more complete by optimizing the pressure and holding time of the pressurized autoclave.
[0037] Step 4, placing the porous carbon on a crucible with silicon particles on the bottom, adding another layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, placing the crucible in a vacuum resistance furnace for reaction infiltration, the reaction infiltration vacuum degree is below 10Pa, the reaction infiltration sintering temperature is 1450-1650°C, the insulation time is 10-60min, and the furnace is cooled to room temperature to obtain the silicified graphite material.
[0038] In step 4, the porous carbon is embedded with silicon particles, which is helpful for the infiltration of liquid silicon. The vacuum degree of the reaction infiltration is controlled below 10Pa. Optimizing the reaction infiltration sintering temperature can effectively promote the infiltration of liquid silicon and produce highly dense silicified graphite.
[0039] The silicified graphite is prepared by reactive infiltration, which has a simple process, low sintering temperature, fast sintering speed, and short preparation cycle, and can effectively reduce the preparation cost.
[0040] In this method, spherical graphite is mixed with nano carbon black. Since the nano carbon black particles have high purity, small particle size, and large specific surface area, the spherical graphite can be well coated to form a dense nano carbon black layer on the particle surface. Since the silicon-carbon reaction is very intense, the spherical graphite without the addition of nano carbon black is difficult to be retained in the reaction infiltration, and the carbon phase content is low, while the carbon source with the addition of nano carbon black is more retained after the reaction infiltration.
[0041] The formed green body is impregnated in resin. The resin immersion under high pressure can well bond the particles. After high-temperature carbonization, the green body becomes very dense. The dense nano-carbon black layer on the surface of the graphite particles reacts preferentially with silicon in the reaction infiltration to form a dense, thinner silicon carbide layer to prevent further reaction of carbon and silicon, effectively protecting the coated graphite particles, thereby realizing the preparation of silicified graphite with high carbon content.
[0042] The carbon content of the obtained silicified graphite is 32.30-39.25 vol.%, and the density is 2.6-2.8 g·cm -3 , open porosity is less than 1%.
[0043] The present invention is further illustrated by means of specific examples below.
[0044] Embodiment 1:
[0045] 1) Spherical graphite and nano carbon black are mechanically mixed in a weight ratio of 80:20, the mixed powder is placed in a mold, and a hydraulic press is used for pressing and molding. The pressing pressure is 30 MPa and the holding time is 30 s;
[0046] 2) using phenolic resin as an impregnating agent, placing the green body in an autoclave at a temperature of 25° C., pressurizing it to 0.7 MPa, using negative pressure to absorb the phenolic resin into it, maintaining the pressure and impregnating it for 5 hours, then releasing the pressure to take out the green body, cleaning the surface and drying it, to obtain the green body after impregnation and drying;
[0047] 3) The impregnated and dried green body is placed in an atmosphere tube furnace and carbonized at 800°C for 3 hours under nitrogen protection;
[0048] 4) placing the porous carbon on a crucible with silicon particles on the bottom, adding another layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, placing the crucible in a vacuum resistance furnace for reactive infiltration, the reactive infiltration vacuum degree is below 10 Pa, the reactive infiltration sintering temperature is 1500°C, the insulation time is 15 min, the size of the silicon particles is 0.5-4 mm, and the weight of the silicon particles is twice the total weight of the green body.
[0049] The carbon content of the silicified graphite material prepared by this process is 34.36 vol.% and the density is 2.75 g cm -3 , open porosity is less than 1%.
[0050] Embodiment 2:
[0051] 1) Spherical graphite and nano carbon black are mechanically mixed in a weight ratio of 85:15, the mixed powder is placed in a mold, and a hydraulic press is used for pressing and molding. The pressing pressure is 35 MPa and the holding time is 40 s;
[0052] 2) using phenolic resin as an impregnating agent, placing the green body in an autoclave at a temperature of 25° C., pressurizing it to 0.8 MPa, using negative pressure to absorb the phenolic resin into it, maintaining the pressure and impregnating it for 4 hours, then releasing the pressure to take out the green body, cleaning the surface and drying it, to obtain the green body after impregnation and drying;
[0053] 3) The impregnated and dried green body is placed in an atmosphere tube furnace and carbonized at 1100°C for 4 hours under nitrogen protection;
[0054] 4) placing the porous carbon on a crucible with silicon particles on the bottom, adding a layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, placing the crucible in a vacuum resistance furnace for reactive infiltration, the reactive infiltration vacuum degree is below 10 Pa, the reactive infiltration sintering temperature is 1550°C, the insulation time is 10 min, the size of the silicon particles is 0.5-4 mm, and the weight of the silicon particles is twice the total weight of the green body.
[0055] The carbon content of the silicified graphite material prepared by this process is 36.45 vol.% and the density is 2.73 g·cm -3 , open porosity is less than 1%.
[0056] Embodiment 3:
[0057] 1) Spherical graphite and nano carbon black are mechanically mixed in a weight ratio of 90:10, the mixed powder is placed in a mold, and a hydraulic press is used for pressing and molding. The pressing pressure is 40 MPa and the holding time is 30 s;
[0058] 2) using phenolic resin as an impregnating agent, placing the green body in an autoclave at a temperature of 25° C., pressurizing it to 0.8 MPa, using negative pressure to absorb the phenolic resin into it, maintaining the pressure and impregnating it for 5 hours, then releasing the pressure to take out the green body, cleaning the surface and drying it, to obtain the green body after impregnation and drying;
[0059] 3) placing the impregnated and dried green body into an atmosphere tube furnace and carbonizing it at 1000°C for 3 hours under argon protection;
[0060] 4) placing the porous carbon on a crucible with silicon particles on the bottom, adding a layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, placing the crucible in a vacuum resistance furnace for reactive infiltration, the reactive infiltration vacuum degree is below 10 Pa, the reactive infiltration sintering temperature is 1450°C, the insulation time is 35 min, the size of the silicon particles is 0.5-4 mm, and the weight of the silicon particles is twice the total weight of the green body.
[0061] The carbon content of the silicified graphite material prepared by this process is 39.25 vol.% and the density is 2.68 g·cm -3 , open porosity is less than 1%.
[0062] The obtained products were characterized by field emission scanning electron microscopy (FESEM). Figure 1 This is a backscattered photo of the product. It can be clearly seen that a large amount of black carbon phase is preserved. No obvious pores are found inside the sample, and the sample is very dense.
[0063] Embodiment 4:
[0064] 1) Spherical graphite and nano carbon black are mechanically mixed in a weight ratio of 95:5, the mixed powder is placed in a mold, and a hydraulic press is used for pressing and molding. The pressing pressure is 40 MPa and the holding time is 20 s;
[0065] 2) using phenolic resin as an impregnating agent, placing the green body in an autoclave at a temperature of 35° C., pressurizing it to 0.6 MPa, using negative pressure to absorb the phenolic resin into it, maintaining the pressure and impregnating it for 2 hours, then releasing the pressure to take out the green body, cleaning the surface and drying it, to obtain the green body after impregnation and drying;
[0066] 3) The impregnated and dried green body is placed in an atmosphere tube furnace and carbonized at 1200°C for 2 hours under argon protection conditions;
[0067] 4) placing the porous carbon on a crucible with silicon particles on the bottom, adding a layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, placing the crucible in a vacuum resistance furnace for reactive infiltration, the reactive infiltration vacuum degree is below 10 Pa, the reactive infiltration sintering temperature is 1650°C, the insulation time is 40 min, the size of the silicon particles is 0.5-4 mm, and the weight of the silicon particles is twice the total weight of the green body.
[0068] The carbon content of the silicified graphite material prepared by this process is 32.30 vol.% and the density is 2.76 g cm -3 , open porosity is less than 1%.
[0069] Comparative Example 1
[0070] Spherical graphite was directly used as the carbon source for the reaction without adding nano carbon black. Other process parameters were the same as those in Example 1. The carbon content of the silicified graphite material finally obtained was 24.10 vol.%.
[0071] The obtained products were characterized by field emission scanning electron microscopy (FESEM). Figure 2 This is a backscattered photo of the product. It can be clearly seen that not much black carbon phase remains. Figure 1 It can be seen that the carbon phase content of the silicified graphite composite material prepared in Comparative Example 1 is significantly less than that in Example 3.
[0072] From the comparison between Examples 1 to 4 and Comparative Example 1, it can be seen that the silicified graphite material prepared by the present invention is very dense, with a density of 2.6 to 2.8 g·cm -3 , the open porosity is less than 1%. The carbon content of the silicified graphite material is not less than 32.30 vol.%, and the carbon content of the silicified graphite material is significantly higher than that of the silicified graphite in Comparative Example 1, wherein Example 1 is increased by 42.57% compared with Comparative Example 1; Example 2 is increased by 51.24% compared with Comparative Example 1; Example 3 is increased by 62.86% compared with Comparative Example 1; and Example 4 is increased by 34.02% compared with Comparative Example 1. The silicified graphite material prepared by the present invention is a graphite material with high carbon content and excellent performance, which can be widely used in chemical industry, metallurgy, environmental protection, national defense, aerospace, nuclear energy and other fields.
[0073] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.
Claims
1. A method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation, characterized in that: The following steps are involved: (1) mechanically mixing spherical graphite and nano carbon black in a mass ratio of 80-95%:5-20%, and pressing the uniformly mixed powder to obtain a green body; (2) Immersing the green body in phenolic resin under pressure, cleaning the surface and then drying it; (3) carbonizing the impregnated and dried green body at high temperature under a protective atmosphere to obtain porous carbon; (4) placing the porous carbon on a crucible with silicon particles on the bottom, adding another layer of silicon particles on the upper surface of the porous carbon so that the porous carbon is completely embedded in the silicon particles, and performing reaction infiltration, sintering, heat preservation, and cooling under vacuum and high temperature to obtain silicified graphite material; The carbon content of silicified graphite is 32.30~39.25 vol.%, and the density is 2.6~2.8 g·cm -3 , open porosity is less than 1%.
2. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The pressure of powder pressing is 30~40 MPa, and the holding time is 20~40 s.
3. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The green body is immersed in phenolic resin under pressure of 0.6-0.8 MPa and the holding time is 2-6 h.
4. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The protective atmosphere was nitrogen or argon.
5. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The heating rate during carbonization is 1 ℃ / min, the carbonization temperature is 800~1200 ℃, and the holding time is 2~4 h.
6. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The reaction infiltration sintering temperature is 1450~1650 ℃, and the holding time is 10~60 min.
7. The method for preparing high carbon silicified graphite based on nano carbon black and resin impregnation according to claim 1, characterized in that: The vacuum degree of reactive infiltration is below 10 Pa.
8. A high carbon silicified graphite prepared by the method according to any one of claims 1 to 7 through impregnation of nano carbon black and resin.