Manufacturing method of directional electromagnetic steel sheet

By using a uniformly dispersed annealing separator of metal compounds for final annealing during the manufacturing process of directional electromagnetic steel sheets, the problem of increased iron loss caused by inhibitor residue was solved, and stable production of directional electromagnetic steel sheets with low iron loss and high magnetic flux density was achieved.

CN116745444BActive Publication Date: 2026-11-17JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280010404.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-21
Filing Date
2022-01-20
Publication Date
2026-11-17
Estimated Expiration
2042-01-20

AI Technical Summary

Technical Problem

In the existing technology, inhibitors such as Ti, Zr, Hf, V, Nb, and Ta remain in the directional electromagnetic steel plate, which hinders the movement of magnetic domain walls and increases iron loss. Moreover, existing purification methods cannot effectively remove these elements, resulting in increased iron loss.

Method used

The final annealing is carried out using a uniformly dispersed annealing agent of metal compounds. The purification of Ti, Zr, Hf, V, Nb and Ta is promoted by oxidation. The specific methods include hot rolling, cold rolling, decarburization annealing, coating of annealing agent and final annealing. Metal compounds such as SnO2 and MoO3 are used to control the particle size and distribution.

Benefits of technology

Effective purification of inhibitors was achieved, enabling the stable manufacture of directional electromagnetic steel plates with excellent magnetic properties, reducing iron loss and increasing magnetic flux density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116745444B_ABST
    Figure CN116745444B_ABST
Patent Text Reader

Abstract

This invention provides a method for stably manufacturing directional electromagnetic steel sheets with excellent magnetic properties by effectively purifying inhibitors. The method for manufacturing the directional electromagnetic steel sheet uses a steel billet containing a specified amount of one or more of Ti, Zr, Hf, V, Nb, and Ta, and adds 1 to 10 parts by mass of a metal compound annealing separating agent relative to 100 parts by mass of MgO, so that the ratio of metal compound particles with a particle size of 1 μm or larger on the steel sheet surface is 0.0010 particles / μm. 2 The coating process will proceed as follows.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing a directional electromagnetic steel sheet, and more particularly to a method for stabilizing the manufacture of a directional electromagnetic steel sheet with excellent magnetic properties by promoting the purification of Ti, Zr, Hf, V, Nb, and Ta as inhibitors. Background Technology

[0002] Directional electromagnetic steel sheets are mainly used as soft magnetic materials for transformer cores, requiring low iron loss and high magnetic flux density as their magnetic properties. This type of directional electromagnetic steel sheet is manufactured by integrating a {110}<001> orientation, known as the Goss orientation, into the steel sheet structure using a secondary recrystallization phenomenon.

[0003] Furthermore, as a method to improve the integration of this Goss orientation, secondary recrystallization is typically controlled by using precipitates called inhibitors, such as MnS, MnSe, and AlN.

[0004] However, in recent years, the demand for directional electromagnetic steel sheets with low iron loss and high magnetic flux density has been increasing due to energy conservation goals. As a method for manufacturing such directional electromagnetic steel sheets, methods using Nb or similar substances as inhibitors have been proposed, for example, in Patent Documents 1 and 2. Nb or similar substances can enhance the inhibition of grain growth and improve the integration of Goss orientation.

[0005] Here, the inhibitor needs to be removed (purified) from the steel, but as a method to promote the purification of the inhibitor, for example, Patent Document 3 proposes a method to promote the purification of nitrogen by reducing the nitrogen partial pressure during purification annealing.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent Application Publication No. 6-25747

[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-115421

[0010] Patent Document 3: Japanese Patent Application Publication No. 9-143562 Summary of the Invention

[0011] As mentioned above, when using inhibitors, if the inhibitors remain in the product, they hinder the movement of magnetic domain walls and increase iron loss. Therefore, it is necessary to remove the inhibitors from the steel by decomposing them (purification) after a secondary recrystallization annealing during the final annealing process and then performing a purification annealing at high temperature.

[0012] However, when Ti, Zr, Hf, V, Nb, or Ta (hereinafter also referred to as Nb, etc.) are used as inhibitors, as described in Patent Documents 1 and 2, there is a problem that they cannot be purified. That is, Nb, etc., which decompose at high temperatures, precipitate again, and this precipitate increases iron loss.

[0013] Furthermore, in the method described in the aforementioned Patent Document 3, there is a problem that even if nitrogen can be purified, Nb and other substances cannot be purified, resulting in increased iron loss.

[0014] The present invention advantageously solves the above-mentioned problems, and its object is to provide, in particular, a method for stably manufacturing directional electromagnetic steel sheets with excellent magnetic properties by effectively purifying inhibitors such as Nb.

[0015] In order to solve the above problems, the inventors conducted repeated and in-depth research, and as a result, they discovered that by using a uniformly dispersed annealing separating agent of metal compounds for final annealing, the oxidation of Ti, Zr, Hf, V, Nb and Ta can be promoted, thereby promoting their purification.

[0016] This invention was developed based on the above insights. Specifically, the main elements of this invention are as follows.

[0017] 1. A method for manufacturing a directional electromagnetic steel sheet, characterized by comprising a series of steps including: hot rolling a steel billet, cold rolling once or twice or more with intermediate annealing, decarburizing annealing, coating with an annealing separating agent, and final annealing, wherein the steel billet contains, by mass percent, C: 0.01-0.1%, Si: 2.0-5.0%, and Mn: 0.01-1%, and further contains, in total, 0.0010-0.0100% of any two or more of Ti, Zr, Hf, V, Nb, and Ta, with the remainder being Fe and unavoidable impurities.

[0018] The above-mentioned annealing separating agent consists of 1 to 10 parts by mass of a metal compound added relative to 100 parts by mass of MgO, with the ratio of particles with a diameter of 1 μm or larger in the above-mentioned metal compound on the steel plate surface being 0.0010 particles / μm. 2 Apply the above-mentioned annealing separating agent as follows.

[0019] 2. The method for manufacturing directional electromagnetic steel sheet according to 1 above, characterized in that the metal compound is any one or more of an oxide, hydroxide, nitrate and sulfate selected from Ti, Cr, Mo, W, Mn, Zn, Sn, Pb, Sb and Bi.

[0020] 3. The method for manufacturing the directional electromagnetic steel sheet according to 1 or 2 above, characterized in that the steel billet further contains, by mass %, any one or more of the following: B: 0.0001-0.005%, N: 0.002-0.01%, Al: 0.004-0.04%, P: 0.005-0.1%, S: 0.002-0.03%, Cr: 0.01-0.5%, Ni: 0.01-1.5%, Cu: 0.01-0.5%, Se: 0.002-0.03%, Mo: 0.005-0.1%, Sn: 0.005-0.5%, Sb: 0.005-0.5%, and Bi: 0.001-0.05%.

[0021] According to the present invention, even when one or more of Ti, Zr, Hf, V, Nb and Ta are used as inhibitors, the purification can be promoted by using an annealing separator in which the metal compound is uniformly dispersed, and the directional electromagnetic steel sheet with excellent magnetic properties can be stably manufactured. Attached Figure Description

[0022] Figure 1 It is in 10 seconds -1 and 15s -1 The graph compares the dispersion state of SnO2 under stirring conditions with varying shear rates. Detailed Implementation

[0023] The following describes the experiment that led to the development of this invention.

[0024] A steel billet containing, by mass percent: 0.03% C, 0.004% N, 0.007% Al, 3.2% Si, 0.06% Mn, and further containing 0.0070% Nb as an inhibitor, with the remainder consisting of Fe and unavoidable impurities, was heated at 1380°C for 30 minutes, followed by hot rolling, then cold rolling, and then intermediate annealing at 1050°C for 1 minute, followed by further cold rolling to produce a cold-rolled sheet with a thickness of 0.23 mm. This cold-rolled sheet was then subjected to decarburization annealing at 840°C for 2 minutes in a moist hydrogen atmosphere.

[0025] Then, for the 11 cold-rolled sheets after decarburization annealing, as shown in Table 1, 6 of them were treated with an annealing separating agent containing 5 parts by mass of SnO2 relative to 100 parts by mass of MgO, and the remaining 5 were treated with an annealing separating agent using MgO. Each annealing separating agent was applied to the surface of the cold-rolled sheet after stirring with varying shear rates. After secondary recrystallization annealing at 850°C for 50 hours, purification annealing was performed at 1200°C for 5 hours in a dry hydrogen atmosphere. A phosphate-based coating was then applied, followed by planarization annealing at 850°C for 1 minute to prepare test pieces. The magnetic properties of these test pieces were then measured, and Nb was analyzed after removing the coating.

[0026] It should be noted that magnetic measurements were performed according to JIS C2550, and compositional analysis was performed using emission spectroscopy. Furthermore, when using an annealing separating agent without added SnO2, the measurements were performed in the same manner as described above.

[0027] The results of all measurements are marked in Table 1.

[0028] [Table 1]

[0029] Table 1

[0030]

[0031] As shown in the table, with the addition of SnO2, especially at 15s... -1 When stirred at the above shear rate, Nb is less than 10 ppm by mass (0.0010% by mass), which promotes purification.

[0032] The details of the reason for this enhanced purification are not yet clear, but the inventors have considered the following.

[0033] In secondary recrystallization annealing, Nb is known to precipitate as NbN, which strengthens the force inhibiting grain growth in the steel sheet structure by the inhibitor. In the higher-temperature purification annealing, it decomposes, and N and Nb dissolve separately. Here, if SnO2 is added during this purification annealing, Nb2O5 is more stable than SnO2. Therefore, it is assumed that the following reaction occurs on the surface of the steel sheet, thereby oxidizing Nb and proceeding with purification.

[0034] 4Nb + 5SnO2 → 2Nb2O5 + 5Sn

[0035] Furthermore, it is believed that the oxidation reaction results in the generation of an activity gradient of Nb, which diffuses and allows Nb to enter the membrane and annealing separator in the form of Nb2O5, thus promoting the purification.

[0036] It should be noted that, in order to evaluate the dispersion state of SnO2, an annealing separating agent was coated onto the steel plate, and after sintering, a scanning electron microscope was used to select a 750 μm area on its surface. 2 The observation was conducted at a magnification of 2000x, with approximately 10 fields of view in a field of view of about the left and right.

[0037] After adding SnO2 to the annealing separator, the results were observed after 10 seconds. -1 and 15s -1 The results of SnO2 dispersion under stirred conditions with a shear rate are shown in the figure. Figure 1 .

[0038] As shown in the figure, SnO2 particles with a diameter greater than 1 μm are ubiquitous at slow shear rates. Conversely, such particles are almost invisible at high shear rates. Specifically, at 10 s... -1 Under stirring conditions at a shear rate, the ratio of SnO2 particles with a diameter greater than 1 μm is 0.0080 particles / μm. 2 Left and right, in contrast, at 15s -1 Under shear rate stirring conditions, this ratio is 0.0010 particles / μm. 2 the following.

[0039] Based on these results, it is believed that during stirring after the addition of SnO2, under slow shear rates, SnO2 aggregates and its distribution becomes uneven, with the ratio of SnO2 particles larger than 1 μm not reaching 0.0010 particles / μm. 2 Therefore, it is believed that the oxidation of Nb becomes uneven, and the purification will not be promoted.

[0040] Next, the composition of the annealing separator of the present invention will be described.

[0041] In this invention, metal compounds such as SnO2 are important components for promoting the purification of steel plates, and their effect is insufficient when their content is less than 1 part by mass relative to MgO: 100 parts by mass. On the other hand, if the content exceeds 10 parts by mass, the MgO ratio decreases, and the coating properties, and even the magnetic properties, deteriorate. Therefore, in this invention, the range of 1 to 10 parts by mass is limited.

[0042] The aforementioned metal compounds of the present invention are decomposed by elements used as inhibitors. If the metal in the metal compound is an oxide, hydroxide, nitrate, or sulfate, these metal compounds are preferred. It is believed that the element used as an inhibitor, replacing the metal of the metal compound, enters the coating and annealing separating agent in a form that promotes the purification.

[0043] It should be noted that, more specifically, the aforementioned metal compound is any one or more of an oxide, hydroxide, nitrate, and sulfate selected from Ti, Cr, Mo, W, Mn, Zn, Sn, Pb, Sb, and Bi.

[0044] In addition, in order to improve the film properties and magnetic properties, conventionally known oxides, hydroxides, borates, carbonates, nitrates, phosphates, sulfates, and halides of Li, Na, Mg, Al, Si, K, Ca, Ti, V, Fe, Co, Ni, Cu, Sr, Ba, and lanthanum can be added to the annealing separating agent.

[0045] It should be noted that these compounds can be used alone or in combination. When using this compound, the preferred content is in the range of 0.01 to 15 parts by mass relative to MgO: 100 parts by mass. If less than 0.01 parts by mass, sufficient effect will not be obtained; on the other hand, if more than 15 parts by mass, the film formation will be excessively promoted, or the aforementioned inhibitory force will be excessively enhanced, leading to deterioration of magnetic properties.

[0046] Next, the composition of the steel billet will be explained.

[0047] Carbon (C) is an important element for improving texture. If its content is less than 0.01% by mass, sufficient effect cannot be obtained. On the other hand, if it exceeds 0.1% by mass, decarburization becomes difficult, leading to deterioration of magnetic properties. Therefore, in this invention, the content is limited to a range of 0.01 to 0.1% by mass.

[0048] Si is an important element for increasing resistivity and improving eddy current loss. If the content is less than 2.0% by mass, sufficient effect cannot be obtained. On the other hand, if it exceeds 5.0% by mass, cold rollability deteriorates. Therefore, in this invention, the range is limited to 2.0 to 5.0% by mass.

[0049] Like Si, Mn increases resistivity and improves eddy current loss. It is also an important element for improving hot rollability, but its effect is insufficient if its content is less than 0.01% by mass. On the other hand, if it exceeds 1% by mass, it causes a γ-phase transition, deteriorating magnetic properties. Therefore, in this invention, the content is limited to a range of 0.01% to 1% by mass.

[0050] Ti, Zr, Hf, V, Nb, and Ta are important elements for enhancing the aforementioned suppression force and improving magnetic properties, but sufficient effects cannot be obtained when their combined content is less than 0.0010% by mass. On the other hand, if the content exceeds 0.0100% by mass, it becomes difficult to perform the purification. Therefore, in this invention, the total content of any one or more of Ti, Zr, Hf, V, Nb, and Ta is limited to the range of 0.0010 to 0.0100% by mass.

[0051] Furthermore, in this invention, MnS, MnSe, and AlN, commonly used in directional electromagnetic steel sheets, can be used as inhibitors. When using MnS or MnSe, it is preferable to add 0.01–1% by mass of Mn and 0.002–0.03% by mass of S or 0.002–0.03% by mass of Se. On the other hand, when using AlN, it is preferable to add 0.004–0.04% by mass of Al and 0.002–0.01% by mass of N. It should be noted that the above inhibitors can be used alone or in combination.

[0052] In addition to the above-mentioned components, for the purpose of improving magnetic properties, one or more of the following components may be appropriately added by weight: B: 0.0001-0.005%, P: 0.005-0.1%, Cr: 0.01-0.5%, Ni: 0.01-1.5%, Cu: 0.01-0.5%, Mo: 0.005-0.1%, Sn: 0.005-0.5%, Sb: 0.005-0.5%, and Bi: 0.001-0.05%.

[0053] Next, the manufacturing method of the directional electromagnetic steel plate of the present invention will be described.

[0054] The steel billet, adjusted to the above-mentioned preferred composition, is hot-rolled according to a known method, annealed as needed, and then cold-rolled once or twice with intermediate annealing to achieve the final plate thickness. Further decarburization annealing is then performed, followed by coating with an annealing separating agent containing 1 to 10 parts by weight of a metal compound relative to 100 parts by weight of MgO. Here, in this invention, the stirring method is not particularly limited. For example, it is preferable to use a stirring blade and adjust the shear rate by changing its rotation speed, or to change the discharge pressure when using a static mixer. It should be noted that this stirring is preferably performed at a speed of 15 seconds. -1 The stirring was performed at the above shear rate. This is because, when observed from the surface of the steel plate, the ratio of metal compound particles with a diameter greater than 1 μm is 0.0010 particles / μm. 2 It should be noted that the particle ratio of the aforementioned metal compound is preferably 0.0005 particles / μm. 2 Below. On the other hand, this lower limit is not specifically limited and can be 0 per μm. 2 Furthermore, a shear rate of 20 s is more preferably specified. -1 That's all. On the other hand, there is no specific upper limit, but industrially it is 300 seconds. -1 about.

[0055] Furthermore, after decarburization annealing, nitriding treatment can be performed as needed to improve magnetic properties.

[0056] Then, after secondary recrystallization annealing, purification annealing is carried out, followed by insulating coating, planarization annealing and magnetic domain refinement treatment as needed, to produce directional electromagnetic steel sheet as the final product.

[0057] It should be noted that in the manufacturing method of the present invention, items not described in this specification can be manufactured using conventional methods.

[0058] Example

[0059] [Example 1]

[0060] A steel billet containing, by mass percent, 0.03% C, 0.004% N, 0.007% Al, 3.2% Si, 0.06% Mn, 0.0050% Nb, with the remainder consisting of Fe and unavoidable impurities, is heated to 1380°C for 30 minutes, hot-rolled, further cold-rolled, and then intermediate-annealed at 1050°C for 1 minute, followed by another cold-rolling to produce a 0.23 mm cold-rolled sheet. This sheet is then decarburized and annealed at 840°C for 2 minutes in a wet hydrogen atmosphere to produce a decarburized annealed sheet. In this decarburized annealed plate, various oxides listed in Table 2 as metal compounds are added relative to MgO: 100 parts by mass. After coating with a stirred annealing separating agent at the shear rate listed in Table 2, a second recrystallization annealing is performed at 850°C for 50 hours, followed by a purification annealing at 1200°C for 5 hours. Then, a phosphate-based coating is applied, and planarization annealing is performed at 850°C for 1 minute to prepare a test piece.

[0061] Then, the magnetic properties of the test piece were measured, and after further removal of the coating, Nb analysis was performed. It should be noted that the magnetic properties were measured according to JIS C2550, and the compositional analysis was performed using emission spectroscopy.

[0062] All measurement and analysis results are marked in Table 2.

[0063]

[0064] As shown in the table, when using the present invention, the amount of Nb is sufficiently reduced (purified) while the magnetic properties are improved.

[0065] [Example 2]

[0066] For steel billets containing the various compositions listed in Table 3, slab heating was performed at 1380°C for 30 minutes, followed by hot rolling, then further cold rolling, intermediate annealing at 1050°C for 1 minute, and finally cold rolling again to produce a 0.23 mm cold-rolled sheet. This sheet was then decarburized and annealed at 840°C for 2 minutes in a moist hydrogen atmosphere to produce a decarburized annealed sheet. For this decarburized annealed sheet, 5 parts by mass of MoO3 as a metallic compound were added relative to 100 parts by mass of MgO, and the coating was applied for 15 seconds. -1 After being subjected to a stirred annealing separating agent at a shear rate, a second recrystallization annealing was performed at 850°C for 50 hours, followed by a purification annealing at 1200°C for 5 hours. Then, a phosphate-based coating was applied, and planarization annealing was performed at 850°C for 1 minute to prepare test pieces. It should be noted that the ratio of particles with a diameter greater than 1 μm in any test piece was 0.0010 [particles / μm]. 2 〕the following.

[0067] Then, the magnetic properties of the test piece were measured, and after further removal of the coating, compositional analysis was performed. It should be noted that the magnetic properties were measured according to JIS C2550, and the compositional analysis was performed using emission spectroscopy.

[0068] All measurement and analysis results are marked in Table 3.

[0069]

[0070] As shown in the table, when using the present invention, magnetic properties are improved while sufficiently reducing (purifying) the elements.

Claims

1. A method for manufacturing a directional electromagnetic steel plate, characterized in that, The process includes the following steps: hot rolling of a steel billet, followed by one or more cold rolling processes with intermediate annealing, decarburization annealing, coating with an annealing separating agent, and final annealing. The steel billet contains, by mass percent, 0.01–0.1% C, 2.0–5.0% Si, and 0.01–1% Mn, and also contains 0.0010–0.0100% of any two or more of Ti, Zr, Hf, V, Nb, and Ta as inhibitors. The remainder consists of Fe and unavoidable impurities. During the final annealing, a secondary recrystallization annealing is performed followed by purification annealing. The annealing separating agent is composed of 1-10 parts by mass of a metal compound added relative to 100 parts by mass of MgO, such that the ratio of particles with a diameter of 1 μm or larger in the metal compound on the surface of the steel plate is 0.0010 particles / μm. 2 The annealing separating agent described above is applied below. The metal compound is decomposed by the element used as the inhibitor.

2. The method for manufacturing a directional electromagnetic steel plate according to claim 1, characterized in that, The metal compound is any one or more of the oxides, hydroxides, nitrates and sulfates selected from at least one of Ti, Cr, Mo, W, Mn, Zn, Sn, Pb, Sb and Bi.

3. The method for manufacturing a directional electromagnetic steel plate according to claim 1 or 2, characterized in that, The steel billet, by mass percent, further contains any two or more of the following: B: 0.0001–0.005%, N: 0.002–0.01%, Al: 0.004–0.04%, P: 0.005–0.1%, S: 0.002–0.03%, Cr: 0.01–0.5%, Ni: 0.01–1.5%, Cu: 0.01–0.5%, Se: 0.002–0.03%, Mo: 0.005–0.1%, Sn: 0.005–0.5%, Sb: 0.005–0.5%, and Bi: 0.001–0.05%.

Citation Information

Patent Citations

  • Manufacture of thin high magnetic flux density grain-oriented silicon steel sheet

    JP1994025747A

  • Production of aluminum-containing grain oriented silicon steel sheet excellent in magnetic property and shape of steel sheet end

    JP1997143562A

  • Method for producing grain-oriented electrical steel sheet excellent in productivity

    JP2008115421A

  • Process for producing grain-oriented electromagnetic steel sheet with excellent core loss characteristics

    CN103781920A

  • Annealing separating agent for grain oriented electrical steel sheet having uniform glass film and excellent magnetic properties and method of manufacturig the same

    WO2008047999A1