Inkjet ink composition, recorded matter, inkjet recording method and inkjet recording system

By using specific structural compounds and hyperbranched acrylate oligomers in inkjet inks, combined with multifunctional acrylates and gelling agents, the problem of viscosity increase and particle size variation of inkjet inks in high temperature and high humidity environments is solved. , achieving both hardness and adhesion and improving stability.

CN116769356BActive Publication Date: 2024-10-18KONICA MINOLTA INC

Patent Information

Application Number
CN202310253427.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2024-10-18
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

Existing inkjet inks are prone to increase in viscosity, change in particle size and produce precipitates in high temperature and high humidity environments, making it difficult to achieve both hardness and adhesion, and the inkjet head filter is prone to clogging.

Method used

The inkjet ink composition formed by using compounds with specific structures and hyperbranched acrylate oligomers or polymers, combined with specific multifunctional acrylates and gelling agents, is cured by active energy rays or heat to inhibit hydrolysis and Precipitates are produced.

Benefits of technology

It achieves inkjet ink with good stability in high temperature and high humidity environments, has both sufficient hardness and adhesion, suppresses viscosity increase and particle size change, and extends the service life of the inkjet head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116769356B_ABST
    Figure CN116769356B_ABST
Patent Text Reader

Abstract

The present invention provides an inkjet ink composition, a recorded object, an inkjet recording method and a recording system that can have sufficient hardness and adhesion as a recorded object, suppress the increase in viscosity during long-term storage and retention, and suppress the change in particle size and the generation of precipitates. The inkjet ink composition of the present invention is an inkjet ink composition that is cured by active energy rays or heat, wherein the inkjet ink composition contains: a compound having a structure represented by the general formula (1) or its salt (A), a hyperbranched acrylate oligomer or polymer (B). [Chemical Formula 1] In the general formula (1), X represents a substituent having at least one selected from acryloyl, methacryloyl, allyl, vinyl and their derivatives at the terminal. Q represents an oxygen atom or NR4, and R4 represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. R1 represents an unsubstituted alkylene group having 1 to 6 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an inkjet ink composition, a recorded object, an inkjet recording method and an inkjet recording system, and more particularly to an inkjet ink composition which has sufficient hardness and adhesion as a recorded object, suppresses an increase in viscosity during long-term storage or retention, and suppresses fluctuations in particle size and generation of precipitates. Background Art

[0002] In order to protect the circuit pattern on the printed wiring board of the printed circuit board, ink is applied and cured to form an insulating film (solder resist film). As a method for forming the solder resist film, for example, an inkjet method is known, in which inkjet ink (hereinafter referred to as "ink") is applied, cured by light, and then cured by heat.

[0003] Patent document 1 discloses an inkjet ink for resist containing a photopolymerizable compound having an acidic group. As the photopolymerizable compound having an acidic group, a carboxyl group, a phosphoric acid group, and a sulfonic acid group are used. However, when a photopolymerizable compound having a phosphoric acid group or a sulfonic acid group is used, the viscosity and particle size of the ink are easily increased due to the aggregation of the pigment, and particularly when the ink bag or the inkjet head is retained at a high temperature, there is a problem of easily causing the variation of the ejection amount and the clogging of the inkjet head filter. In addition, when a photopolymerizable compound having a carboxyl group is used, compared with a phosphoric acid group or a sulfonic acid group, the viscosity and particle size are not easy to increase, but there is a problem of difficulty in obtaining sufficient hardness and adhesion as a resist film.

[0004] Patent Document 2 discloses a technology of an adhesive composition comprising an acrylic resin, an ionic compound, and a polymeric carbodiimide. However, the carbodiimide compound has a mechanism of inhibiting hydrolysis by reacting with a carboxylic acid, and therefore, when applied to an inkjet ink, there is a problem that the viscosity of the ink is easily increased.

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2020-37645

[0008] [Patent Document 2] Japanese Patent Application Publication No. 2018-178468 Summary of the invention

[0009] [Technical problem solved by the invention]

[0010] The present invention has been completed in view of the above-mentioned problems and conditions, and the technical problem to be solved is to provide an inkjet ink composition, recorded matter, inkjet recording method and inkjet recording system that can have sufficient hardness and adhesion as a recorded matter (such as an anti-etching film), suppress the increase in viscosity during long-term storage and retention, and suppress the change in particle size and the generation of precipitates.

[0011] [Technical means to solve the problem]

[0012] In order to solve the technical problem, the inventors found that, in the process of studying the causes of the problem, among the photopolymerizable compounds having a carboxyl group, by using a compound having a specific structure, it is not easy to cause pigment aggregation, and sufficient hardness and adhesion as a recorded object (such as a resist film) can be obtained. However, when using the compound having the specific structure, it was found that in a high temperature and high humidity environment, hydrolyzate precipitation occurs, causing clogging of the inkjet head filter.

[0013] Therefore, the present inventors have achieved the present invention by making it contain a compound having a specific structure and a hyperbranched acrylate oligomer or polymer, thereby achieving sufficient hardness and adhesion as a recorded material, suppressing the increase in viscosity during long-term storage and retention, suppressing the change in particle size, suppressing hydrolysis even in a high temperature and high humidity environment, and suppressing the generation of precipitates.

[0014] That is, the technical problem of the present invention is solved by the following means.

[0015] 1. An inkjet ink composition, which is an inkjet ink composition that is cured by active energy rays or heat, wherein:

[0016] The inkjet ink composition contains: a compound having a structure represented by the following general formula (1) or a salt thereof (A); and

[0017] Hyperbranched acrylate oligomer or polymer (B).

[0018] [Chemical formula 1]

[0019] General formula (1)

[0020]

[0021] [In the general formula (1), X represents a substituent having at least one selected from the group consisting of acryloyl, methacryloyl, allyl, vinyl and derivatives thereof at the terminal.

[0022] Q represents an oxygen atom or NR 4 , R 4 represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group.

[0023] R 1 represents an unsubstituted alkylene group having 1 to 6 carbon atoms.]

[0024] 2. The inkjet ink composition according to item 1, wherein

[0025] In the general formula (1), X represents an acryloyl group or a methacryloyl group.

[0026] 3. The inkjet ink composition according to item 1 or 2, wherein

[0027] In the general formula (1), Q represents an oxygen atom.

[0028] 4. The inkjet ink composition according to any one of items 1 to 3, wherein

[0029] In the general formula (1), R 1 It represents an unsubstituted alkylene group having 1 or 2 carbon atoms.

[0030] 5. The inkjet ink composition according to any one of items 1 to 4, further comprising:

[0031] A polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B).

[0032] 6. The inkjet ink composition according to item 5, wherein

[0033] The polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B) is caprolactam-modified dipentaerythritol hexaacrylate.

[0034] 7. The inkjet ink composition according to any one of items 1 to 6, further comprising:

[0035] A (meth)acrylate compound (D) having a ClogP value within a range of 4.0 to 7.0.

[0036] 8. The inkjet ink composition according to any one of items 1 to 7, further comprising a gelling agent (E).

[0037] 9. The inkjet ink composition according to any one of items 1 to 8, which is used as an inkjet ink for forming a solder resist pattern in a printed circuit board.

[0038] 10. A recorded matter obtained by curing the inkjet ink composition according to any one of items 1 to 9 by active energy rays or heat.

[0039] 11. An inkjet recording method, which is an inkjet recording method using an inkjet ink composition, wherein:

[0040] Using the inkjet ink composition according to any one of items 1 to 9, and

[0041] The inkjet recording method has:

[0042] A step of ejecting the inkjet ink composition from an inkjet head to drop onto a recording medium; and

[0043] A step of curing the inkjet ink composition that has landed on a recording medium by active energy rays or heat.

[0044] 12. An inkjet recording system, which is an inkjet recording system using an inkjet ink composition, wherein:

[0045] Using the inkjet ink composition according to any one of items 1 to 9, and

[0046] The inkjet recording system has:

[0047] An inkjet head for ejecting the inkjet ink composition, an active energy ray irradiation unit for irradiating the inkjet ink composition landed on a recording medium with active energy rays, and a heating unit for heating the inkjet ink composition irradiated with the active energy rays.

[0048] [Effects of the Invention]

[0049] The method of the present invention can provide an inkjet ink composition, recorded matter, inkjet recording method and inkjet recording system which have both sufficient hardness and adhesion as a recorded matter, suppress the increase in viscosity during long-term storage and retention, and suppress the change in particle size and the generation of precipitates.

[0050] Although the expression mechanism and action mechanism of the effect of the present invention are not yet clear, they are presumed as follows.

[0051] Generally, when a compound having an ester bond (or an amide bond) is heated in the presence of water and an acid, hydrolysis occurs and an alcohol (or an amine) and a carboxylic acid are produced. This reaction is an equilibrium reaction.

[0052] The compound having a structure represented by the general formula (1) or its salt (A) in the present invention has a dicarboxylic acid structure and is coordinated to the metal substrate and adheres more firmly than general carboxylic acid acrylates. On the other hand, the dicarboxylic acid generated by hydrolysis has low solubility in the monomer and is easily precipitated.

[0053] On the other hand, the hyperbranched acrylate oligomer or polymer (B) also has an acrylate structure, and unreacted hydroxyl groups may remain in the molecule, or may be hydrolyzed to generate hydroxyl groups. In addition, since it has a branched structure, it is considered that a plurality of hydroxyl groups may be contained in one molecule.

[0054] Therefore, by using the compound or its salt (A) and the hyperbranched acrylate oligomer or polymer (B) in combination, the hydroxyl concentration in the ink can be increased, and the equilibrium of the hydrolysis reaction of the compound or its salt (A) can be shifted to the ester side, thereby suppressing hydrolysis.

[0055] Furthermore, since the hyperbranched acrylate oligomer or polymer (B) has a branched structure, it may contain a plurality of hydroxyl groups in one molecule, and it is considered that hydrolysis can be more effectively suppressed than the combined use of a hydroxyl-containing compound other than the hyperbranched acrylate oligomer or polymer (B). DETAILED DESCRIPTION

[0056] The inkjet ink composition of the present invention is an inkjet ink composition that is cured by active energy rays or heat, wherein the inkjet ink composition contains: a compound having a structure represented by the following general formula (1) or a salt thereof (A); and a hyperbranched acrylate oligomer or polymer (B).

[0057] [Chemical formula 2]

[0058] General formula (1)

[0059]

[0060] In the general formula (1), X represents a substituent having at least one selected from the group consisting of acryloyl group, methacryloyl group, allyl group, vinyl group and derivatives thereof at the terminal.

[0061] Q represents an oxygen atom or NR 4 , R 4 represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group.

[0062] This feature is a common or corresponding technical feature of the following embodiments.

[0063] As an embodiment of the present invention, in the general formula (1), X represents an acryloyl group or a methacryloyl group, which is preferred from the viewpoint of improving the reactivity of the compound having a structure represented by the general formula (1) or a salt thereof (A) and improving the adhesion.

[0064] Furthermore, from the viewpoint of reducing the viscosity of the ink and improving the ink jetting suitability, the total number of carbon atoms of the substituent represented by X is preferably 50 or less, more preferably 30 or less.

[0065] In the general formula (1), Q represents an oxygen atom, which is preferred from the viewpoint of improving adhesion.

[0066] In addition, in the general formula (1), R 1 An unsubstituted alkylene group having 1 or 2 carbon atoms is preferred from the viewpoint of improving the adhesion.

[0067] From the viewpoint of improving the hardness of the coating film, it is preferred that the coating film further contains a polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B).

[0068] The polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B) is preferably caprolactam-modified dipentaerythritol hexaacrylate from the viewpoint of suppressing the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A) and further improving the acid resistance and alkali resistance.

[0069] It is preferred to further contain a (meth)acrylate compound (D) having a ClogP value within a range of 4.0 to 7.0 from the viewpoint of reducing the water absorption of the ink and inhibiting the hydrolysis of the compound having a structure represented by the general formula (1) or a salt thereof (A).

[0070] It is preferred to further contain a gelling agent (E) from the viewpoint that the ink on the recording medium can be temporarily fixed in a gelled state and the wetting and spreading of the ink can be suppressed. In addition, by reducing the water absorption of the ink, the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A) can be suppressed.

[0071] The inkjet ink composition of the present invention is suitable for use as an inkjet ink for forming a solder resist pattern used in a printed circuit board. In addition, the inkjet ink composition of the present invention is suitable for use in a recorded object cured by active energy rays or heat.

[0072] The inkjet recording method of the present invention is an inkjet recording method using an inkjet ink composition, wherein the inkjet ink composition is used, and the inkjet recording method comprises: a step of ejecting the inkjet ink composition from an inkjet head to make it fall on a recording medium; and a step of curing the inkjet ink composition that falls on the recording medium by active energy rays or heat.

[0073] This makes it possible to obtain a recorded material having excellent hardness and adhesion, and to suppress an increase in viscosity during long-term storage or retention, thereby suppressing a change in particle size and the generation of precipitates.

[0074] The inkjet recording system of the present invention is an inkjet recording system using an inkjet ink composition, wherein the inkjet ink composition is used, and the inkjet recording system comprises: an inkjet head that ejects the inkjet ink composition, an active energy ray irradiation unit that irradiates the inkjet ink composition that falls onto a recording medium with active energy rays, and a heating unit that heats the inkjet ink composition irradiated with the active energy rays.

[0075] This makes it possible to obtain a recorded material having excellent hardness and adhesion, and to suppress an increase in viscosity during long-term storage or retention, thereby suppressing a change in particle size and the generation of precipitates.

[0076] Hereinafter, the present invention and its constituent elements as well as specific embodiments and forms for implementing the present invention will be described. It should be noted that in the present application, "to" means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0077] [Inkjet ink composition of the present invention]

[0078] The inkjet ink composition of the present invention is an inkjet ink composition that is cured by active energy rays or heat, wherein the inkjet ink composition contains: a compound having a structure represented by the following general formula (1) or a salt thereof (A); and a hyperbranched acrylate oligomer or polymer (B).

[0079] [Chemical formula 3]

[0080] General formula (1)

[0081]

[0082] [In the general formula (1), X represents a substituent having at least one selected from the group consisting of acryloyl, methacryloyl, allyl, vinyl and derivatives thereof at the terminal.

[0083] Q represents an oxygen atom or NR 4 , R 4 represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. 1 represents an unsubstituted alkylene group having 1 to 6 carbon atoms.]

[0084] The inkjet ink composition of the present invention functions as an insulating film (solder resist) by being applied on a substrate and cured by light or heat in various fields such as metal processing, electronic circuits, printed circuit boards, platemaking, semiconductor fields, and color filters. In addition, since it can be removed with an alkali after photocuring, it also functions as an etching resist used when forming an etching pattern on a substrate.

[0085] Specifically, on a conductive oxide film of copper, zinc, etc. formed on a substrate, the inkjet ink composition of the present invention is patterned by inkjet printing, and then cured by light to form a resist film. Then, the oxide film not covered by the resist film is removed by an acid-based etching solution, and the resist film covering the oxide film is removed by an alkali, thereby forming a fine circuit or pattern.

[0086] In addition to the above applications, it is mainly used to pattern a film having both adhesion and hardness on a substrate having an inorganic surface such as metal or glass.

[0087] The inkjet ink composition of the present invention is an ink composition that can be cured by active light.

[0088] “Active light” refers to light that can impart energy to generate initiating species in the ink composition by irradiation, and includes α rays, γ rays, X-rays, ultraviolet rays, electron rays, etc. Among them, ultraviolet rays and electron rays are preferred, and ultraviolet rays are more preferred, from the viewpoint of curing sensitivity and easy availability of equipment.

[0089] [1. A compound having a structure represented by the general formula (1) or a salt thereof (A)]

[0090] The inkjet ink composition of the present invention (hereinafter also referred to as "ink") contains the compound having a structure represented by the general formula (1) or a salt thereof (A), so that it can have both hardness and adhesion as a recorded object, and can suppress changes in viscosity and particle size during long-term storage and retention.

[0091] In the general formula (1), from the viewpoint of improving the reactivity of the compound having a structure represented by the general formula (1) or a salt thereof (A) and improving the adhesion, X preferably represents an acryloyl group or a methacryloyl group.

[0092] Furthermore, from the viewpoint of reducing the viscosity of the ink and improving the ink jetting suitability, the total number of carbon atoms of the substituent represented by X is preferably 50 or less, more preferably 30 or less.

[0093] In the general formula (1), Q represents an oxygen atom, which is preferred from the viewpoint of improving adhesion.

[0094] In addition, in the general formula (1), R 1 An unsubstituted alkylene group having 1 or 2 carbon atoms is preferred from the viewpoint of improving the adhesion.

[0095] Furthermore, it is preferred that the compound having a structure represented by the general formula (1) is not a salt from the viewpoint of improving compatibility with other monomers and the hydrophobicity of the ink and inhibiting the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A).

[0096] Specific examples of the compound having a structure represented by the general formula (1) or a salt thereof are shown below, but the present invention is not limited thereto.

[0097] [Chemical formula 4]

[0098]

[0099] [Chemical formula 5]

[0100]

[0101] The higher the content of the compound having the structure represented by the general formula (1) or its salt (A), the better the hardness and adhesion. If it is too much, it acts as an acid catalyst to promote its own hydrolysis. Therefore, it is preferably in the range of 1 to 50% by mass, and more preferably in the range of 3 to 20% by mass, relative to the total ink.

[0102] [2. Hyperbranched acrylate oligomer or polymer (B)]

[0103] The ink of the present invention contains a hyperbranched acrylate oligomer or polymer (B), thereby suppressing the hydrolysis of the compound having a structure represented by the general formula (1) or a salt thereof (A), and suppressing the precipitation.

[0104] The hyperbranched acrylate oligomer of the present invention is an acrylate oligomer having a hyperbranched (hyperbranched chain) structure.

[0105] In the present invention, the "oligomer" refers to a compound having a monomer bonding number (polymerization degree) in the range of 2 to 10 and a weight average molecular weight in the range of 500 to 15,000.

[0106] In the present invention, the term "polymer" refers to a compound having a monomer bonding number (polymerization degree) of 11 or more and a weight average molecular weight of more than 10,000.

[0107] The polymer of the present invention is preferably a polymer of the above-mentioned oligomer, for example.

[0108] In the present invention, "hyperbranched structure" refers to a dendritic compound having multiple branch points in one molecule, for example, an AB structure having a total of three or more substituents of two types in one molecule. 2 The self-condensation of the type molecules, or as two molecules (A 2 Type, B 3 A 2 +B 3 Synthesized by method.

[0109] Therefore, the hyperbranched structures of the present invention include dendritic structures (tree-like structures), star structures and grafted structures.

[0110] Examples of commercially available hyperbranched acrylate oligomers include V#1000 (manufactured by Osaka Organic Chemical Industry Co., Ltd.), CN2302, CN2303, CN2304 (manufactured by Sartomer), SP1106 (manufactured by MIWON), 6361-100, 6363 (manufactured by Changxing Science Industry Co., Ltd.), etc. These may be used alone or in combination of two or more.

[0111] The higher the content of the hyperbranched acrylate oligomer or polymer (B), the more helpful it is to inhibit the hydrolysis of the compound having the structure represented by the general formula (1) or its salt (A). If it is too much, the viscosity of the ink is too high and it is difficult to eject through the inkjet head. Therefore, it is preferably in the range of 5 to 50% by mass, more preferably in the range of 10 to 30% by mass, relative to the total mass of the ink.

[0112] [3. Multifunctional (meth)acrylate (C) which is not a hyperbranched acrylate oligomer or polymer and has three or more (meth)acryloyl groups]

[0113] The ink of the present invention can further improve the hardness of the coating film by preferably containing a polyfunctional (meth)acrylate (C) which is not a hyperbranched acrylate oligomer or polymer and has three or more (meth)acryloyl groups (hereinafter referred to as "polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups").

[0114] The multifunctional (meth)acrylate (C) having three or more (meth)acryloyl groups generally has a large curing shrinkage and is easily impaired in adhesion to the substrate. By using it in combination with the compound having a structure represented by the general formula (1) or its salt (A), the necessary adhesion can be maintained while greatly improving the hardness of the coating film. In addition, from the viewpoint of improving the hardness of the coating film, the multifunctional (meth)acrylate (C) having three or more (meth)acryloyl groups preferably has five or more (meth)acryloyl groups, and more preferably has six or more.

[0115] The ink of the present invention may contain only one type of the polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups, or may contain two or more types of polyfunctional (meth)acrylate.

[0116] Examples of (meth)acrylates having three (meth)acryloyl groups (also referred to as "trifunctional (meth)acrylates") include trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tri(meth)acrylates in which three hydroxyl groups of a triol obtained by adding 3 or more ethylene oxide or propylene oxide to 1 mol of trimethylolpropane are substituted with (meth)acryloyloxy groups.

[0117] Examples of the (meth)acrylate having four (meth)acryloyl groups (also referred to as “tetrafunctional (meth)acrylate”) include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol ethoxy tetra(meth)acrylate, and pentaerythritol tetra(meth)acrylate.

[0118] Examples of the (meth)acrylate having five (meth)acryloyl groups (also referred to as “pentafunctional (meth)acrylate”) include dipentaerythritol penta(meth)acrylate and the like.

[0119] Examples of the (meth)acrylate having six (meth)acryloyl groups (also referred to as “hexafunctional (meth)acrylate”) include dipentaerythritol hexa(meth)acrylate and the like.

[0120] In addition, the (meth)acrylate may be a modified product.

[0121] Examples of the modified (meth)acrylate include ethylene oxide-modified (meth)acrylates including ethylene oxide-modified trimethylolpropane tri(meth)acrylate, ethylene oxide-modified pentaerythritol tetra(meth)acrylate, and the like, propylene oxide-modified (meth)acrylates including propylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified pentaerythritol tetra(meth)acrylate, and the like, caprolactone-modified (meth)acrylates including caprolactone-modified trimethylolpropane tri(meth)acrylate, and caprolactone-modified (meth)acrylates including caprolactone-modified dipentaerythritol hexa(meth)acrylate, and the like.

[0122] In particular, caprolactam-modified dipentaerythritol hexaacrylate is particularly preferred because it can reduce the water absorption of the ink, thereby inhibiting the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A), thereby improving acid and alkali resistance.

[0123] Examples of commercially available products of the (meth)acrylate include M500 (pentafunctional acrylate, manufactured by Sartomer Co., Ltd.) and M600 (hexafunctional acrylate, manufactured by Sartomer Co., Ltd.).

[0124] Examples of commercially available products of caprolactam-modified dipentaerythritol hexaacrylate include DPC A20, DPCA30, DPCA60, and DPCA120 (all of which are hexafunctional acrylates, manufactured by Nippon Kayaku Co., Ltd.).

[0125] The content of the polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups is preferably in the range of 5 to 50% by mass, more preferably in the range of 10 to 30% by mass, based on the entire ink.

[0126] [4. (Meth)acrylate (D) having a ClogP value within a range of 4.0 to 7.0]

[0127] The ink of the present invention preferably contains a (meth)acrylate (D) having a ClogP value within a range of 4.0 to 7.0, from the viewpoint of reducing the water absorption of the ink and inhibiting the hydrolysis of the compound having a structure represented by the general formula (1) or a salt thereof (A).

[0128] Examples of the (meth)acrylate (D) having a ClogP value within a range of 4.0 to 7.0 include propoxylated (2) neopentyl glycol diacrylate (molecular weight 471, ClogP 4.9), 1,10-decanediol dimethacrylate (molecular weight 310, ClogP 5.75), tricyclodecane dimethanol diacrylate (molecular weight 304, ClogP 4.69), and tricyclodecane dimethanol dimethacrylate (molecular weight 332, ClogP 5.12).

[0129] Examples of commercially available products of the (meth)acrylate (D) having a ClogP value within the range of 4.0 to 7.0 include SR834 (manufactured by Sartomer) (tricyclodecane dimethanol dimethacrylate), NK ESTETR DOD-N (manufactured by Shin-Nakamura Chemical Co., Ltd.) (1,10-decanediol dimethacrylate), NK ESTETR NOD-N (manufactured by Shin-Nakamura Chemical Co., Ltd.) (1,9-nonanediol dimethacrylate), NK ESTETR A-DOD-N (manufactured by Shin-Nakamura Chemical Co., Ltd.) (1,10-decanediol diacrylate), and NK ESTETR A-NOD-N (manufactured by Shin-Nakamura Chemical Co., Ltd.) (1,10-nonanediol diacrylate).

[0130] Furthermore, from the viewpoint of suppressing the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A), it is more preferred that the (meth)acrylate (D) having a ClogP value within the range of 4.0 to 7.0 is contained in the range of 10 to 40% by mass based on the total ink.

[0131] Here, the "logP value" in the present application refers to a coefficient indicating the affinity of an organic compound for water and 1-octanol.

[0132] The 1-octanol / water partition coefficient P is the distribution equilibrium when a trace compound is dissolved as a solute in a two-phase solvent of 1-octanol and water, and is the ratio of the equilibrium concentrations of the compound in each solvent, and is expressed by their logarithms logP relative to the base 10. That is, the "logP value" is the logarithm of the 1-octanol / water partition coefficient, and is known as an important parameter indicating the hydrophilicity and hydrophobicity of a molecule.

[0133] "ClogP value" is a logP value calculated by calculation. The ClogP value can be calculated by a fragmentation method, an atomic proximity method, etc. More specifically, in order to calculate the ClogP value, a fragmentation method described in the literature (C. Hansch and A. Leo, "Substituent Constants for Correlation Analysis in Chemistry and Biology" (John Wiley & Sons, New York, 1969) or the following commercially available software packages 1 or 2 can be used.

[0134] Software package 1: MedChem Software (Release 3.54, August 1991, Medicinal Chemistry Project, Pomona College, Claremont, CA)

[0135] Software package 2: Chem Draw Ultra ver. 8.0. (April 2003, CambridgeSoft Corporation, USA)

[0136] The numerical value of the ClogP value described in the specification of this application etc. is the "ClogP value" calculated using Software Package 2.

[0137] [5.Polymerization initiator]

[0138] The ink of the present invention can be cured by radical polymerization or ion polymerization. In the present invention, a radical polymerization initiator is preferably used as the polymerization initiator.

[0139] The ink of the present invention may contain only one type of polymerization initiator, or may contain two or more types of polymerization initiators.

[0140] Examples of the radical polymerization initiator include an α-cleavage type radical polymerization initiator (also referred to as a “Norrish I type polymerization initiator”) and a hydrogen abstraction type radical polymerization initiator (also referred to as a “Norrish II type polymerization initiator”).

[0141] The content of the α-cleavage type radical polymerization initiator is preferably in the range of 0.3 to 6% by mass relative to the total mass of the ink of the present invention. In addition, the content of the hydrogen abstraction type radical polymerization initiator is preferably in the range of 0.5 to 10% by mass relative to the total mass of the ink of the present invention.

[0142] An α-cleavage type free radical polymerization initiator is an initiator that cleaves upon photoexcitation and directly provides initiating free radicals.

[0143] In addition, the hydrogen abstraction type radical polymerization initiator is a photopolymerization initiator that is activated by active energy rays (such as ultraviolet rays) and generates radicals by abstracting hydrogen from the second compound, and the second compound becomes the actual initiating radical. This second compound is called a polymerization synergist or a coinitiator.

[0144] Both the α-cleavage type radical polymerization initiator and the hydrogen abstraction type radical polymerization initiator may be used alone or in combination in the present invention.

[0145] Examples of the α-cleavage type radical polymerization initiator include acetophenone-based initiators, benzoin-based initiators, acylphosphine oxide-based initiators, and benzyl and methyl phenylglyoxylates.

[0146] Examples of acetophenone initiators include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl-phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propane-1-one and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.

[0147] Examples of the benzoin-based initiator include benzoin, benzoin methyl ether and benzoin isopropyl ether.

[0148] Examples of the acylphosphine oxide initiator include 2,4,6-trimethylbenzoindiphenylphosphine oxide and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.

[0149] Examples of the hydrogen abstraction type free radical initiator include benzophenone-based initiators, thioxanthone-based initiators, aminobenzophenone-based initiators, 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, and camphorquinone.

[0150] Examples of the benzophenone initiator include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acryloyl benzophenone, 3,3',4,4'-tetrakis(tert-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone.

[0151] Examples of the thioxanthone-based initiator include 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone.

[0152] Examples of the aminobenzophenone-based initiator include Michler's ketone and 4,4'-diethylaminobenzophenone.

[0153] [6. Inhibitor]

[0154] The ink of the present invention preferably further contains a polymerization inhibitor. By containing a polymerization inhibitor, the adhesion between a plurality of curable compounds can be reduced.

[0155] In the present invention, the “polymerization inhibitor” includes all compounds added to inhibit a polymerization reaction during the preparation of an ink containing a polymerizable compound or during storage after adjustment.

[0156] In the present invention, various conventionally known polymerization inhibitors can be used. As the polymerization inhibitor, any one of an N-oxyl radical polymerization inhibitor, a phenolic polymerization inhibitor containing an o-tert-butyl group, or a polymerization inhibitor having two or more aromatic rings can be included, and these are more preferred from the viewpoint of effect expression.

[0157] Among these, it is more preferable to contain an N-oxyl radical polymerization inhibitor from the viewpoint of adhesion to a printed wiring board.

[0158] In the ink of the present invention, the content of the polymerization inhibitor is preferably in the range of 0.05 to 0.5% by mass relative to the total mass of the ink.

[0159] [6-1. N-oxyl radical inhibitor]

[0160] Examples of the N-oxyl radical-based polymerization inhibitor include 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl radical (TEMPO), 4-hydroxy-2,2,6,6-tetramethyl-piperidine-N-oxyl radical, 4-oxo-2,2,6,6-tetramethyl-piperidine-N-oxyl radical, 4-methoxy-2,2,6,6-tetramethyl-piperidine-N-oxyl radical, 4-acetoxy-2,2,6,6-tetramethyl-piperidine-N-oxyl radical, and IRGASTAB (registered trademark) UV10 (manufactured by BASF).

[0161] [6-2. Phenol inhibitors]

[0162] Examples of the phenolic polymerization inhibitor include 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,4,6-tri-tert-butylphenol, 2,6-di-tert-butyl-p-cresol (butylated hydroxytoluene: BHT), 4-methoxyphenol, and 2-methoxy-4-methylphenol.

[0163] [6-3. Quinone type polymerization inhibitor]

[0164] Examples of the quinone-based polymerization inhibitor include hydroquinone, methoxyhydroquinone, benzoquinone, 1,4-naphthoquinone, and p-tert-butylcatechol.

[0165] [6-4. Amine inhibitors]

[0166] Examples of the amine-based polymerization inhibitor include alkylated diphenylamine, N,N′-diphenyl-p-phenylenediamine, and phenothiazine.

[0167] [6-5. Other polymerization inhibitors]

[0168] In addition, copper dithiocarbamate-based polymerization inhibitors such as dimethyl copper dithiocarbamate, diethyl copper dithiocarbamate, and dibutyl copper dithiocarbamate can be mentioned.

[0169] These may contain only one kind or two or more kinds.

[0170] Among them, preferred are N-oxyl free radical and quinone type polymerization inhibitors, preferably 4-hydroxy-2,2,6,6-tetramethylpiperidinium-N-oxyl free radical (TEMPO), 2,6-di-tert-butyl-p-cresol (butylated hydroxytoluene: BHT), and 2,4-di-tert-butylphenol. As the polymerization inhibitor having two or more aromatic rings, naphthoquinone and the like are preferred.

[0171] [7. Gelling agent]

[0172] The ink of the present invention preferably further contains a gelling agent.

[0173] By including a gelling agent, the ink on the recording medium can be temporarily pinned to a gel state, and the wetting and spreading of the ink can be suppressed. In addition, by reducing the water absorption of the ink, the hydrolysis of the compound having a structure represented by the general formula (1) or its salt (A) can be suppressed.

[0174] The gelling agent preferably crystallizes at a temperature lower than or equal to the gelling temperature of the ink.

[0175] The “gelation temperature” refers to a temperature at which, when a composition that has been solified or liquidified by heating is cooled, the gelling agent undergoes a phase change from a sol to a gel, and the viscosity of the composition changes rapidly.

[0176] Specifically, the composition in a solubilized or liquidized state can be cooled while measuring the viscosity using a viscoelasticity measuring apparatus (eg, MCR300, manufactured by ANTON PAAR), and the temperature at which the viscosity suddenly rises can be defined as the gelation temperature of the composition.

[0177] In the present invention, when the gelling agent is crystallized in the ink, a structure containing a polymerizable compound (compounds participating in polymerization such as multifunctional compound A, acrylate oligomer, monomer, etc.) is formed in the three-dimensional space formed by the crystallized plate-like gelling agent, i.e., a so-called card-house structure. In order to form the card-house structure, the polymerizable compound dissolved in the ink is preferably miscible with the gelling agent.

[0178] Examples of gelling agents suitable for forming a card-house structure include aliphatic ketones, aliphatic esters, petroleum waxes, vegetable waxes, animal waxes, mineral waxes, hydrogenated castor oil, modified waxes, higher fatty acids, higher alcohols, hydroxystearic acid, fatty acid amides containing N-substituted fatty acid amides and special fatty acid amides, higher amines, sucrose fatty acid esters, synthetic waxes, dibenzylidene sorbitol, dimer acids, and dimer diols.

[0179] Among them, from the viewpoint of improving the pinning property, aliphatic ketones, aliphatic esters, higher fatty acids and higher alcohols having a hydrocarbon group having 9 to 25 carbon atoms are preferred.

[0180] The gelling agent may be contained alone or in combination of two or more.

[0181] [7-1. Aliphatic ketones]

[0182] Examples of the aliphatic ketone include ditetracosyl ketone, dibehenyl ketone, distearyl ketone, diicosyl ketone, dipalmityl ketone, dilauryl ketone, dimyristyl ketone, myristylpalmityl ketone, and palmitylstearyl ketone.

[0183] [7-2. Aliphatic esters]

[0184] Examples of the aliphatic ester include fatty acid esters of monoalcohols such as behenyl behenate, eicosyl eicosate, and oleyl palmitate; and fatty acid esters of polyalcohols such as glycerol fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, ethylene glycol fatty acid esters, and polyoxyethylene fatty acid esters.

[0185] Examples of commercially available products of the aliphatic esters include EMALEX (registered trademark) series manufactured by NIHON-EMULSION, and RIKEMAL (registered trademark) series and POEM (registered trademark) series manufactured by RIKEN Vitamin Co., Ltd.

[0186] [7-3. Higher fatty acids]

[0187] Examples of higher fatty acids include behenic acid, arachidic acid, stearic acid, palmitic acid, myristic acid, lauric acid, oleic acid, and erucic acid.

[0188] [7-4. Higher alcohols]

[0189] Examples of higher alcohols include stearyl alcohol and behenyl alcohol.

[0190] [7-5. Suitable gelling agent]

[0191] In the present invention, the gelling agent is particularly preferably an aliphatic ketone represented by the following general formula (G1) or an aliphatic ester represented by the following general formula (G2).

[0192] General formula (G1): R 1 -CO-R 2

[0193] (In the general formula (G1), R 1 and R 2 Each independently represents an alkyl group containing a straight chain part having 12 to 26 carbon atoms and optionally containing a branched chain. 1 and R 2 Can be the same or different.)

[0194] General formula (G2): R 3 -COO-R 4

[0195] (In the general formula (G2), R 3 and R 4 Each independently represents an alkyl group containing a straight chain part having 12 to 26 carbon atoms and optionally containing a branched chain. 3 and R 4 Can be the same or different.)

[0196] In the general formulae (G1) and (G2), the number of carbon atoms in the linear or branched hydrocarbon group is 12 or more, and thus the aliphatic ketone represented by the general formula (G1) and the aliphatic ester represented by the general formula (G2) have higher crystallinity and more sufficient space is generated in the card-house structure. Therefore, the polymerizable compound is easily and fully contained in the space, and the pinning property of the ink is improved.

[0197] In addition, by having a straight-chain or branched hydrocarbon group with a carbon number of 26 or less, the melting point of the aliphatic ketone represented by the general formula (G1) or the aliphatic ester represented by the general formula (G2) will not rise excessively, that is, the melting point can be made to a temperature that is easy to handle, and there is no need to overheat the ink when spraying the ink.

[0198] Examples of the aliphatic ketone represented by the general formula (G1) include: ditetracosyl ketone (carbon number: 23, 24), dibehenyl ketone (carbon number: 21, 22), distearyl ketone (carbon number: 17, 18), dieicosyl ketone (carbon number: 19, 20), dipalmityl ketone (carbon number: 15, 16), dimyristyl ketone (carbon number: 13, 14), dilauryl ketone (carbon number: 11, 12), lauryl myristyl ketone (carbon number: 13, 14), dilauryl ketone (carbon number: 11, 12), and dilauryl myristyl ketone (carbon number: 13, 14). Myristyl ketone (carbon number: 11, 14), lauryl palmityl ketone (carbon number: 11, 16), myristyl palmityl ketone (carbon number: 13, 16), myristyl stearyl ketone (carbon number: 13, 18), myristyl behenyl ketone (carbon number: 13, 22), palmityl stearyl ketone (carbon number: 15, 18), palmityl behenyl ketone (carbon number: 15, 22) and stearyl behenyl ketone (carbon number: 17, 22). It should be noted that the number of carbon atoms in parentheses indicates the number of carbon atoms of each of the two hydrocarbon groups separated by the carbonyl group.

[0199] Examples of commercially available products of the aliphatic ketone represented by the general formula (G1) include 18-pentatriacontanon and Hentriacontan-16-on manufactured by ALFA AESER, and KAOWAX T-1 manufactured by Kao Corporation.

[0200] Examples of the aliphatic ester represented by the general formula (G2) include behenyl behenate (carbon number: 21, 22), eicosyl eicosate (carbon number: 19, 20), stearyl stearate (carbon number: 17, 18), palmityl stearate (carbon number: 16, 17), lauryl stearate (carbon number: 12, 17), cetyl palmitate (carbon number: 6, 15), stearyl palmitate (carbon number: 15, 18), Myristyl myristate (carbon number: 13, 14), cetyl myristate (carbon number: 13, 16), octyldodecyl myristate (carbon number: 13, 20), stearyl oleate (carbon number: 17, 18), stearyl erucate (carbon number: 18, 21), stearyl linoleate (carbon number: 17, 18), behenyl oleate (carbon number: 18, 22), and eicosyl linoleate (carbon number: 17, 20). It should be noted that the carbon number in parentheses indicates the carbon number of each of the two hydrocarbon groups divided by the ester group.

[0201] Examples of commercially available products of the aliphatic ester represented by the general formula (G2) include UNISTAR (registered trademark) M-2222SL and SPERMACETI manufactured by NOF Corporation, EXCEPARL (registered trademark) SS and EXCEPARL (registered trademark) MY-M manufactured by Kao Corporation, EMALEX (registered trademark) CC-18 and EMALEX (registered trademark) CC-10 manufactured by NIHON-EMULSION, and AMREPS (registered trademark) PC manufactured by KOKYU AL COHOL KOGYO.

[0202] In the present invention, the content of the gelling agent is preferably in the range of 1 to 10% by mass relative to the total mass of the ink.

[0203] [8. Other ingredients]

[0204] [8-1. Surfactant]

[0205] The ink of the present invention may further contain a surfactant as required.

[0206] Examples of surfactants include anionic surfactants such as dialkyl sulfosuccinates, alkylnaphthalene sulfonates and fatty acid salts, nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols and polyoxyethylene-polyoxypropylene block copolymers, cationic surfactants such as alkylamine salts and quaternary ammonium salts, and polysiloxane and fluorine-based surfactants.

[0207] [8-2. Colorant]

[0208] The ink of the present invention may further contain a colorant as required.

[0209] The colorant may be a pigment or a dye, and a pigment is preferred from the viewpoint of having good dispersibility in the constituent components of the ink and excellent weather resistance.

[0210] The pigment is not particularly limited, and examples thereof include organic pigments or inorganic pigments having the following numbers described in the Color Index.

[0211] In the ink of the present invention, the colorant may be contained in one kind or in two or more kinds, and the color may be adjusted to a desired color.

[0212] The content of the colorant is preferably in the range of 0.1 to 20% by mass, more preferably in the range of 0.2 to 10% by mass, based on the total mass of the ink.

[0213] (pigment)

[0214] 《Red or Magenta Paint》

[0215] Examples of red or magenta pigments include pigment red 3, pigment red 5, pigment red 19, pigment red 22, pigment red 31, pigment red 38, pigment red 43, pigment red 48:1, pigment red 48:2, pigment red 48:3, pigment red 48:4, pigment red 48:5, pigment red 49:1, pigment red 53:1, pigment red 57:1, pigment red 57:2, pigment red 58:4, pigment red 63:1, pigment red 81, pigment red 81:1, pigment red 81:2, pigment red 81:3, pigment red 81:4, pigment red 88, pigment red 104, pigment red 108, and pigment red 1 12. Pigment Red 122, Pigment Red 123, Pigment Red 144, Pigment Red 146, Pigment Red 149, Pigment Red 166, Pigment Red 168, Pigment Red 169, Pigment Red 170, Pigment Red 177, Pigment Red 178, Pigment Red 179, Pigment Red 184, Pigment Red 185, Pigment Red 208, Pigment Red 216, Pigment Red 226, Pigment Red 257, Pigment Violet 3, Pigment Violet 19, Pigment Violet 23, Pigment Violet 29, Pigment Violet 30, Pigment Violet 37, Pigment Violet 50, Pigment Violet 88, Pigment Orange 13, Pigment Orange 16, Pigment Orange 20, Pigment Orange 36 or a mixture thereof, etc.

[0216] Blue or Cyan Pigment

[0217] Examples of blue or cyan pigments include pigments selected from Pigment Blue 1, Pigment Blue 15, Pigment Blue 15:1, Pigment Blue 15:2, Pigment Blue 15:3, Pigment Blue 15:4, Pigment Blue 15:6, Pigment Blue 16, Pigment Blue 17:1, Pigment Blue 22, Pigment Blue 27, Pigment Blue 28, Pigment Blue 29, Pigment Blue 36, and Pigment Blue 60, or mixtures thereof.

[0218] Green Paint

[0219] Examples of the green pigment include pigments selected from Pigment Green 7, Pigment Green 26, Pigment Green 36, and Pigment Green 50, or mixtures thereof.

[0220] Yellow Paint

[0221] Examples of the yellow pigment include pigments selected from Pigment Yellow 1, Pigment Yellow 3, Pigment Yellow 12, Pigment Yellow 13, Pigment Yellow 14, Pigment Yellow 17, Pigment Yellow 34, Pigment Yellow 35, Pigment Yellow 37, Pigment Yellow 55, Pigment Yellow 74, Pigment Yellow 81, Pigment Yellow 83, Pigment Yellow 93, Pigment Yellow 94, Pigment Yellow 95, Pigment Yellow 97, Pigment Yellow 108, Pigment Yellow 109, Pigment Yellow 110, Pigment Yellow 137, Pigment Yellow 138, Pigment Yellow 139, Pigment Yellow 153, Pigment Yellow 154, Pigment Yellow 155, Pigment Yellow 157, Pigment Yellow 166, Pigment Yellow 167, Pigment Yellow 168, Pigment Yellow 180, Pigment Yellow 185, and Pigment Yellow 193, or a mixture thereof.

[0222] Black Pigment

[0223] Examples of the black pigment include pigments selected from Pigment Black 7, Pigment Black 28, and Pigment Black 26, or mixtures thereof.

[0224] 《Examples of Commercially Available Pigments》

[0225] Examples of commercially available pigments include BLACK PIGMENT (manufactured by MIKUNI CORPORATION), CHROMOFINE YELLOW 2080, 5900, 5930, AF-1300, 2700L, CHR OMOFINE ORANGE 3700L, 6730, CHROMOFINE SCARLET 6750, CHR OMOFINE MAGENTA 6880, 6886, 6891N, 6790, 6887, CHROMOFINE VIOLETRE, CHROMOFINE RED 6820, 6830, and CHROMOFINE BLUE. HS-3, 5187, 5108, 5197, 5085N, SR-5020, 5026, 5050, 4920, 4927, 4937, 4824, 4933GN-EP, 4940, 4973, 5205, 5208, 5214, 5221, 5000P, CHRO MOFINE GREEN 2GN, 2GO, 2G-550D, 5310, 5370, 6830, CHROMOFI NE BLACK A-1103, SEIKAFAST YELLOW 10GH, A-3, 2035, 2054, 2200, 2270, 2300, 2400(B), 2500, 2600, ZAY-260, 2700(B), 2770, SEIKA FAST RED 8040, C405(F), CA120, LR-116, 1531B, 8060R, 1547, ZAW-262, 1537B, GY, 4R-4016, 3820, 3891, ZA-215, SEIKAFAST CARMIN E 6B1476T-7, 1483LT, 3840, 3870, SEIKAFAST BORDEAUX 10B-430, SEIKALIGHT ROSE R40, SEIKALIGHTVIOLET B800, 7805, SEIKAFAST MAROON 460N, SEIKAFAST ORANGE 900, 2900, SEIKALIGHTBLUE C718、A612、CYANINE BLUE 4933M, 4933GN-EP, 4940, 4973 (all manufactured by Dainichi Seika Industries, Ltd.; it should be noted that "CHROMOFINE" is a registered trademark of the company);KET YELLOW 401, 402, 403, 404, 405, 406, 416, 424, KET OR ANGE 501, KET RED 301, 302, 303, 304, 305, 306, 307, 308, 309, 310, 336, 337, 338, 346, KET BLUE 101, 102, 103, 104, 105, 106, 111, 118, 124, KET GREEN201 (the above are made by DIC Company); COLORTEX YELLO W 301, 314, 315, 316, P-624, 314, U10GN, U3GN, UNN, UA-414, U263, FINECOL YELLOW T-13, T-05, PIGMENT YELLOW 1705, COLOR TEX ORANGE202, COLORTEX RED 101, 103, 115, 116, D3B, P-625, 102, H-1024, 105C, UFN, UCN, UBN, U3BN, URN, UGN, UG276, U456, U457, 105C, USN, COLORTEX MAROON 601, COLORTEX BRO WN B610N, COLORTEX VIOLET 600, PIGMENT RED 122, COLORTEX BLUE 516, 517, 518, 519, A818, P-908, 510, COLORTEX GREEN 402, 403, COLORTEX BLACK 702, U905 (all manufactured by Sanyo Color Co., Ltd., and it should be noted that "COLORTEX" and "FINECOL" are registered trademarks of the company); LIONOL YEL LOW 1405G, LIONOL BLUE FG7330, FG7350, FG7400G, FG7405G, ES, ESP-S (all manufactured by TOYO INK Co., Ltd., and it should be noted that "LIONOL" is a registered trademark of the company); TONER MAGENTA E02, PERMANENT RUBIN F6B, TONERYELLOW HG, PERMANENT YELLOW GG-02, HOSTAPEAM BLUE B2G (all manufactured by HOECHST INDUSTRY); NOVOPERM P-HG, HOSTAPER M PINK E, HOSTAPERM BLUE B2G (all manufactured by CLARIANT, and it should be noted that "NOVOPERM" and "HOSTAPERM" are registered trademarks of the company);Carbon black #2600, #2400, #2350, #2200, #1000, #990, #980, #970, #960, #950, #850, MCF88, #750, #650, MA600, MA7, MA8, MA11, MA100, MA100R, MA77, #52, #50, #47, #45, #45L, #40, #33, #32, #30, #25, #20, #10, #5, #44, CF9 (all manufactured by Mitsubishi Chemical), etc.;

[0226] "Dispersion of Pigments"

[0227] The pigment can be dispersed by, for example, a ball mill, a sand mill, an attritor, a roll mill, a stirrer, a Henschel mixer, a colloid mill, an ultrasonic homogenizer, a pearl mill, a wet jet mill, a paint shaker, or the like.

[0228] The pigment is preferably dispersed so that the volume average particle size of the pigment particles is preferably within a range of 0.08 to 0.5 μm, and the maximum particle size is preferably within a range of 0.3 to 10 μm, more preferably within a range of 0.3 to 3 μm.

[0229] The dispersion of the pigment is adjusted according to the selection of the pigment, dispersant and dispersion medium, dispersion conditions and filtration conditions.

[0230] Dispersants

[0231] The ink of the present invention may further contain a dispersant to improve the dispersibility of the pigment.

[0232] Examples of dispersants include carboxylic acid esters having a hydroxyl group, salts of long-chain polyaminoamide and high molecular weight acid esters, salts of high molecular weight polycarboxylic acids, salts of long-chain polyaminoamide and polar acid esters, high molecular weight unsaturated acid esters, polymer copolymers, modified polyurethanes, modified polyacrylates, polyether ester type anionic activators, naphthalenesulfonic acid formalin condensate salts, aromatic sulfonic acid formalin condensate salts, polyoxyethylene alkyl phosphates, polyoxyethylene nonylphenyl ethers, and stearylamine acetate, etc. Examples of commercially available dispersants include SOLSPERSE (registered trademark) series manufactured by AVECIA, PB series manufactured by AJINOMOTO FINE-TECHNO, etc.

[0233] 《Dispersing aids》

[0234] The ink of the present invention may further contain a dispersing aid as necessary.

[0235] The dispersing aid can be selected according to the pigment.

[0236] The total content of the dispersant and the dispersing aid is preferably in the range of 1 to 50% by mass relative to the total mass of the pigment.

[0237] 《Dispersion Medium》

[0238] The ink of the present invention may further contain a dispersion medium for dispersing a pigment, if necessary.

[0239] The ink of the present invention may contain a solvent as a dispersion medium. In order to suppress the residual solvent in the formed image, it is preferable to use the above-mentioned monomer (particularly a monomer having a low viscosity) as the dispersion medium.

[0240] [8-3. Other additives]

[0241] The ink of the present invention may further contain a coupling agent, a solvent, etc. as necessary.

[0242] (Coupling agent)

[0243] The ink of the present invention may further contain various coupling agents as needed. By containing a coupling agent, the adhesion to a printed wiring board can be improved.

[0244] Examples of various coupling agents include silane-based, titanium-based, and aluminum-based coupling agents.

[0245] (Solvent)

[0246] The ink of the present invention is preferably solvent-free from the viewpoint of rapid curing and ejection stability, but solvent may be added for the purpose of adjusting the viscosity of the ink.

[0247] [Method for producing the inkjet ink composition of the present invention]

[0248] The ink of the present invention can be prepared by mixing the compound having the structure represented by the general formula (1) or its salt (A), the hyperbranched acrylate oligomer or polymer (B), and any other components under heating. In addition, the obtained mixed solution is preferably filtered with a specific filter. It should be noted that when preparing an ink containing a pigment, it is preferred to prepare a pigment dispersion containing a pigment and a polymerizable compound, and then mix the pigment dispersion and other components. The pigment dispersion may also contain a dispersant.

[0249] The pigment dispersion can be prepared by dispersing the pigment in the polymerizable compound. The pigment can be dispersed using, for example, a ball mill, a sand mill, an attritor, a roller mill, a stirrer, a Henschel mixer, a colloid mill, an ultrasonic homogenizer, a pearl mill, a wet jet mill, a paint stirrer, etc. At this time, a dispersant may also be added.

[0250] [Record of the present invention]

[0251] In the recorded matter of the present invention, the inkjet ink composition of the present invention is cured by active energy rays or heat. That is, the recorded matter of the present invention refers to a recorded matter recorded on a recording medium by an inkjet recording method described later using the inkjet ink composition of the present invention. It should be noted that the cured matter in the present invention refers to a substance obtained by curing the inkjet ink composition of the present invention, and is substantially synonymous with the recorded matter.

[0252] [Inkjet recording method of the present invention]

[0253] In the inkjet recording method of the present invention, the inkjet ink composition of the present invention is used, and the recording method comprises: a step of ejecting the inkjet ink composition from an inkjet head to make it fall on a recording medium; and a step of curing the inkjet ink composition that has fallen on the recording medium by active energy rays or heat.

[0254] In the inkjet method, ink is ejected from an inkjet head and falls on a recording medium. The inkjet method is easy to apply ink only to necessary parts, so it is particularly suitable for forming solder resist patterns and printing text.

[0255] In the step of curing by irradiation with active energy rays, curing may be performed immediately after the step of dropping the ink, or may be performed all at once after the step of dropping the ink is completed.

[0256] The viscosity of the ink of the present invention is relatively high at room temperature (25°C), and it is not easy to wet and spread after falling on the recording medium. Therefore, it is not necessary to cure the ink immediately after falling on the recording medium. The ink can be cured at the same time after being ejected and falling on the recording medium within a certain range. By curing at the same time, ejection defects caused by light leakage can be reduced.

[0257] In the present invention, "all at once irradiating", "all at once heating" and "all at once curing" mean that after a plurality of ink droplets are landed on a recording medium within a certain or specific range, all of the plurality of ink droplets that fall within the certain range are irradiated with active energy rays or heated to be cured. That is, the ink is not cured for each droplet landed on the recording medium, but the ink is landed, irradiated with active energy rays or heated, and cured for a certain or specific range (for example, all the ink required to form a specific image (pattern) is landed) at once.

[0258] Furthermore, it is preferable to form a solder resist film for a printed wiring board by the inkjet recording method of the present invention.

[0259] The inkjet recording method of the present invention is described below. The inkjet recording method of the present invention comprises: (1) ejecting the ink of the present invention from an inkjet head to land on a recording medium; and (2) curing the ink landed on the recording medium by active energy rays or heat.

[0260] [Process of (1)]

[0261] In the step (1), the ink of the present invention is ejected from the nozzles of the inkjet head and is deposited on a recording medium. The recording medium is not particularly limited, but is preferably a printed circuit board.

[0262] The ejection method from the inkjet head may be either an on-demand method or a continuous method.

[0263] The on-demand inkjet head can be any of the electromechanical conversion methods such as single-chamber type, dual-chamber type, curved tube type, piston type, shared pattern type and shared wall type, as well as the electrothermal conversion method such as thermal inkjet type and BUBBLE JET (registered trademark) (BUBBLE JET is a registered trademark of Canon Inc.) type.

[0264] By ejecting ink droplets from the inkjet head in a heated state, ejection stability can be obtained. The temperature of the ink when filled in the inkjet head is preferably in the range of 40 to 100° C., and more preferably in the range of 40 to 90° C. from the viewpoint of further improving ejection stability. In addition, the viscosity of the ink is preferably in the range of 7 to 15 mPa·s at the ejection temperature, and more preferably in the range of 8 to 13 mPa·s.

[0265] When using a sol-gel phase change ink containing a gelling agent, the temperature of the ink when filled in the inkjet head is preferably in the range of (gelling temperature + 10) to (gelling temperature + 30) ° C of the ink. By setting the temperature of the ink in the inkjet head to be above (gelling temperature + 10) ° C, the ink is not gelled in the inkjet head or on the nozzle surface, and sufficient ejection stability can be obtained. In addition, by setting the temperature of the ink to be below (gelling temperature + 30) ° C, the components contained in the ink are prevented from being degraded due to temperature.

[0266] The method for heating the ink is not particularly limited. For example, at least one of the ink supply system such as the ink tank constituting the head carriage, the supply pipe, the ink tank in the front chamber close to the head, the pipe with the filter, and the piezoelectric head can be heated by using a panel heater, a belt heater, or warm water.

[0267] From the viewpoint of recording speed and image quality, the amount of ink droplets during discharge is preferably in the range of 2 to 20 pL.

[0268] The recording medium is not particularly limited, and various metals, glass, ceramics, polyimide films, PET films, etc. can be used. In terms of improving adhesion, it is preferred to include inorganic substances such as metals and glass on the surface. As metals, for example, copper, aluminum, iron, their oxides, etc. can be cited. In addition, it is particularly suitable to use a printed circuit board that includes inorganic substances such as metals and glass on the surface. As an example of a printed circuit board, it is preferred to use a copper-clad laminated plate for high-frequency circuits using materials such as epoxy glass cloth, glass polyimide, epoxy glass cloth / non-woven fabric, epoxy glass cloth / paper, etc., and copper-clad laminated plates of all grades (FR-4, etc.).

[0269] [Process of (2)]

[0270] In step (2), the ink deposited on the recording medium is cured by active energy rays or heat. The ink of the present invention can be cured by only irradiation with active energy rays or only heating. It is preferred to cure by at least irradiation with active energy rays, and more preferably by further heating.

[0271] As the active energy ray, electron beams, ultraviolet rays, α rays, γ rays, X-rays and the like can be used, and ultraviolet rays are preferred.

[0272] The ultraviolet ray irradiation can be performed at a wavelength of 395 nm using, for example, a water-cooled LED manufactured by Phoseon Technology Co., Ltd. By using an LED as a light source, poor curing of the ink due to dissolution of the ink by the radiation heat of the light source can be suppressed.

[0273] The peak illuminance of ultraviolet rays having a wavelength in the range of 370 to 410 nm on the surface of the solder resist film is preferably 0.5 to 10 W / cm 2 In the range of 1 to 5 W / cm 2 From the viewpoint of suppressing radiant heat from irradiating the ink, the amount of light irradiating the solder resist film is preferably less than 1000 mJ / cm 2 .

[0274] The irradiation with the active energy ray is preferably performed between 0.001 and 300 seconds after the ink is applied, and more preferably performed between 0.001 and 60 seconds in order to form a high-definition solder resist film.

[0275] From the viewpoint of suppressing polymerization inhibition caused by oxygen, it is preferred to cure the ink by irradiating the dropped ink with active energy rays in an atmosphere having an oxygen concentration in the range of 0.1 to 10.0% by volume. Furthermore, from the viewpoint of preventing blooming from occurring, it is more preferred that the oxygen concentration be in the range of 0.5 to 8.0% by volume, and even more preferred that it be in the range of 0.5 to 6.0% by volume.

[0276] As a heating method, for example, it is preferable to place the mixture in an oven set at a temperature within a range of 110 to 180° C. for 10 to 90 minutes.

[0277] [Inkjet recording system of the present invention]

[0278] The inkjet recording system of the present invention uses the inkjet ink composition of the present invention and comprises: an inkjet head for ejecting the inkjet ink composition, an active energy ray irradiation unit for irradiating the inkjet ink composition that has landed on a recording medium with active energy rays, and a heating unit for heating the inkjet ink composition irradiated with the active energy rays.

[0279] That is, in the system of the present invention, a recording device and the ink of the present invention are used, wherein the recording device has an inkjet head that ejects an inkjet ink composition, an active energy ray irradiation unit that irradiates the inkjet ink composition that falls onto a recording medium with active energy rays, and a heating unit that heats the inkjet ink composition irradiated with the active energy rays.

[0280] It should be noted that, from the viewpoint of discharge stability and printing accuracy, the recording method of the inkjet recording device is preferably a scanning method.

[0281] The inkjet recording device used in the present invention comprises: an inkjet head that ejects the ink of the present invention onto a recording medium; an active energy ray irradiation unit that irradiates the ink of the present invention landed on the recording medium with active energy rays (e.g., ultraviolet rays) to cure the ink of the present invention; and a heating unit that heats and further cures the ink.

[0282] As types of inkjet recording devices (printers), there are single-pass printers and serial printers. A single-pass printer has a line print head having a length equivalent to the width of the recording medium (the width of the recording medium), and the print head is (substantially) fixed and does not move, and prints in one pass (single pass).

[0283] On the other hand, a serial printer generally performs printing in two or more passes (multi-pass) while the print head reciprocates (shuttle movement) in a direction perpendicular to the conveyance direction of the recording medium.

[0284] In a single-pass printer, a plurality of inkjet heads must be arranged to form a line print head, which requires a relatively large number of inkjet heads. However, in the case of a serial printer, only a small number of recording heads can be used.

[0285] In the present invention, any type of printer may be used, but a serial printer is preferably used.

[0286] [Example]

[0287] The present invention is specifically described below with reference to examples, but the present invention is not limited thereto. It should be noted that, in the following examples, unless otherwise specified, the operation is performed at room temperature (25° C.). In addition, unless otherwise specified, “%” and “part” represent “mass %” and “mass part”, respectively.

[0288] <Preparation of Yellow Pigment Dispersion Liquid Y>

[0289] The following dispersants 1 and 2 and the dispersion medium were placed in a stainless steel beaker, heated and stirred on a heating plate at 65°C for 1 hour to dissolve, and after cooling to room temperature, the following pigments were added, and the mixture was placed in a sealed glass bottle together with 200 g of zirconia beads with a diameter of 0.5 mm.

[0290] After the particles are dispersed by a paint shaker until the desired particle size is achieved, the zirconium oxide beads are removed.

[0291] Dispersant 1: PX4701 (manufactured by BASF) 6.0 parts by mass

[0292] Dispersant 2: Solsperse 22000 (produced by Japan LUBRIZOL Co., Ltd.) 0.3 parts by mass

[0293] Dispersion medium: 61.5 parts by mass of dipropylene glycol diacrylate (containing 0.2% UV-10)

[0294] Pigment: PY185 (manufactured by BASF, PALIOTOL YELLOW D1155) 10.2 parts by mass

[0295] <Preparation of Cyan Pigment Dispersion Liquid C>

[0296] In the preparation of the yellow pigment dispersion Y, the same method as the dispersion Y was carried out except that the dispersant, the dispersion medium and the pigment were changed as follows.

[0297] Dispersant: PX4701 (manufactured by BASF) 7.0 parts by mass

[0298] Dispersion medium: 70 parts by mass of dipropylene glycol diacrylate (containing 0.2% UV-10)

[0299] Pigment: PB15:4 (manufactured by Dainichi Seika, CHROMOFINE (registered trademark) BLUE 6332JC) 23 parts by mass

[0300] The acidic acrylate used in the preparation of the ink described below (used in the ink of the comparative example), the compound having a structure represented by the general formula (1) or a salt thereof (A), a hyperbranched acrylate oligomer or polymer (B), a multifunctional (meth)acrylate (C) which is not a hyperbranched acrylate oligomer or polymer and has three or more (meth)acryloyl groups, a (meth)acrylate (D) having a ClogP value within the range of 4.0 to 7.0, a polymerization initiator, a polymerization inhibitor, a gelling agent, a hydrolysis inhibitor, other monomers, etc., are described below.

[0301] <Acidic acrylate>

[0302] Phosphate acrylate: LIGHTESTER P-2M (manufactured by Kyoeisha Chemical Co., Ltd.)

[0303] [Chemical formula 6]

[0304] Carboxylic acid acrylate 1

[0305]

[0306] Carboxylic acid acrylate 2

[0307]

[0308] <Compound having a structure represented by general formula (1) or a salt thereof (A)>

[0309] A-1: the exemplary compound A-1

[0310] A-2: The exemplary compound A-2

[0311] A-3: The exemplary compound A-3

[0312] <Hyperbranched acrylate oligomer or polymer (B)>

[0313] B-1: CN2304 (manufactured by SARTOMER) (18-functional hyperbranched polyester acrylate)

[0314] B-2: SP1106 (manufactured by MIWON) (18-functional dendritic acrylate)

[0315] B-3: 6361-100 (manufactured by Changxing Chemical Industry Co., Ltd.) (octafunctional hyperbranched polyester acrylate)

[0316] <Multifunctional (meth)acrylate (C) that is not a hyperbranched acrylate oligomer or polymer and has three or more (meth)acryloyl groups>

[0317] C-1: M600 (manufactured by MIWON) (6-functional (meth)acrylate: dipentaerythritol hexaacrylate)

[0318] C-2: M500 (manufactured by MIWON Co., Ltd.) (5-functional (meth)acrylate: dipentaerythritol pentaacrylate)

[0319] C-3: DPCA120 (manufactured by Nippon Kayaku Co., Ltd.) (6-functional (meth)acrylate: caprolactam-modified dipentaerythritol hexaacrylate)

[0320] (Meth)acrylate (D) with a ClogP value in the range of 4.0 to 7.0

[0321] SR834 (manufactured by SARTOMER Co., Inc.) (tricyclodecane dimethanol dimethacrylate) (molecular weight 304, ClogP 4.69)

[0322] NK ESTETR DOD-N (manufactured by Shin-Nakamura Chemical Co., Ltd.) (1,10-decanediol dimethacrylate) (molecular weight 310, ClogP 5.75)

[0323] <Polymerization initiator>

[0324] Type I (Norrish type I) A:

[0325] Omnirad (registered trademark) 907, manufactured by IGM Resins (B.V.)

[0326] Type I (Norrish type I) B:

[0327] Omnirad (registered trademark) 819, manufactured by IGM Resins (B.V.)

[0328] Type II (Norrish type II):

[0329] Speedcure (registered trademark) ITX (manufactured by Lambson)

[0330] <Polymerization inhibitor>

[0331] IRGASTAB (registered trademark) UV-10 (manufactured by BASF)

[0332] <Gelation agent>

[0333] Gelation agent A: EXCEPARL SS (manufactured by Kao Corporation) (aliphatic ester represented by the general formula (G2))

[0334] <Hydrolysis inhibitor>

[0335] Carbodiimide: V02B (manufactured by Nisshinbo Chemical Inc.)

[0336] <Other monomers>

[0337] M222: Dipropylene glycol diacrylate (manufactured by MIWON)

[0338] <Preparation of ink>

[0339] The following components were mixed and filtered using a TEFLON (registered trademark) 3 μm membrane filter manufactured by ADVATEC, to prepare Ink 6.

[0340] <<Compound having a structure represented by general formula (1) or a salt thereof (A)>>

[0341] A-1 10.0 parts by mass

[0342] 《Hyperbranched acrylate oligomer or polymer (B)》

[0343] B-1 20.0 parts by mass

[0344] 《Polymerization Initiator》

[0345] Type I Type A 3.0 parts by mass

[0346] Type I B 3.0 parts by mass

[0347] Type II 2.0 parts by mass

[0348] 《Polymerization Inhibitors》

[0349] IRGASTAB (registered trademark) UV-10 0.1 parts by mass

[0350] Pigment dispersion

[0351] Dispersion liquid Y 0.7 parts by mass

[0352] Dispersion liquid C 0.5 parts by mass

[0353] Other monomers

[0354] The remaining parts of the M222

[0355] In the preparation of ink 6, each ink was prepared in the same manner except that (A), (B), (C), (D), acidic acrylate, gelling agent, hydrolysis inhibitor and other monomers were changed to the types and addition amounts described in Table I.

[0356] In addition, in the preparation of ink, "the remainder" means the amount after excluding the addition amount of various compounds used when the total amount is 100 parts by mass.

[0357] In addition, in Table I, "(A)" is a compound having a structure represented by the general formula (1) or a salt thereof (A), "(B)" is a hyperbranched acrylate oligomer or polymer (B), "(C)" is a multifunctional (meth)acrylate (C) that is not a hyperbranched acrylate oligomer or polymer and has three or more (meth)acryloyl groups, and "(D)" is a (meth)acrylate (D) having a ClogP value in the range of 4.0 to 7.0.

[0358] <Formation of Cured Ink Film by Inkjet Method>

[0359] Each prepared ink was loaded in an inkjet recording device having an inkjet recording head with a piezoelectric inkjet nozzle. Using this device, solder resist patterning was performed on a copper-clad laminate for a printed wiring board (FR-4 thickness 1.6 mm, size 150 mm×95 mm) to obtain a cured film (or cured product).

[0360] The ink supply system consists of an ink tank, ink flow path, a sub-ink tank in front of the inkjet recording head, a pipe with a metal filter, and a piezoelectric head. The ink is heated to 80°C from the ink tank to the nozzle. The piezoelectric head also has a built-in heater to heat the ink temperature in the recording head to 80°C. In the piezoelectric head, nozzles with a nozzle diameter of 22μm and a nozzle resolution of 360dpi are arranged in a zigzag shape to form a nozzle array of 720dpi.

[0361] The inkjet device was used to apply voltage to form dots with a droplet volume of 6.0 pL. A solid pattern of 20 mm × 50 mm was printed on the substrate in a manner such that the thickness was 20 μm. Then, an LED lamp (395 nm, 8 W / cm 2 , water cooling unit) to become 1W / cm 2 、500mJ / cm 2 Then, the coating film was cured by irradiation in a manner of 100° C. Then, the coating film was put into an oven set at 150° C. for 60 minutes to obtain a cured film.

[0362] [evaluate]

[0363] <Viscosity Change>

[0364] The prepared inks were measured for viscosity at 80° C. using Physica MCR 301 (manufactured by Anton Paar) at a shear rate of 1000 (1 / s). Immediately after the preparation, the viscosity was stored at 85° C. for 4 days and then measured, and evaluated based on the following criteria.

[0365] (Benchmark)

[0366] ○Viscosity fluctuation is less than 0.7mPa·s

[0367] △Viscosity fluctuation is 0.7mPa·s or more and less than 1.0mPa·s

[0368] ×Viscosity fluctuation is 1.0 mPa·s or more

[0369] <Average Particle Size Change>

[0370] The average particle size (Z-average) of each ink was measured by dynamic light scattering using ZETASIZER NANO ZSP (manufactured by Malvern). The ink was diluted 200 times and measured at a temperature of 25°C. After the solution was adjusted, the solution was immediately stored at 85°C for 4 days and then measured, and evaluated according to the following criteria.

[0371] (Benchmark)

[0372] ○The average particle size variation is less than 15nm

[0373] △The average particle size varies from 15nm to less than 30nm

[0374] × Average particle size variation is 30 nm or more

[0375] <Adhesion>

[0376] The solid pattern print sample was cut into a checkerboard pattern according to the cross-cut method of JIS standard K5600 on the cured film, and an adhesive tape was attached. The adhesive tape was peeled off and the peeling state of the cured film was observed.

[0377] (Benchmark)

[0378] ◎: The adhesion remaining rate is 100%.

[0379] ○: The adhesion residual rate is 80% or more and less than 100%.

[0380] △: The adhesion residual rate is 60% or more and less than 80%.

[0381] ×: The adhesion residual rate is less than 60%.

[0382] <Pencil Hardness>

[0383] The surface pencil hardness of the prepared printed sample of the solid pattern was measured according to the method described in JIS standard K-5400.

[0384] <Precipitation>

[0385] About 10 g of the prepared ink was placed in a transparent heat-resistant tube and stored at 85° C. for 1 day, 4 days, 1 week, and 2 weeks, and the increase of precipitates was visually observed before and after storage.

[0386] (Benchmark)

[0387] ◎: No increase in precipitates was observed even after 2 weeks.

[0388] ○: No increase in precipitates was observed after 1 week, but an increase in precipitates was observed after 2 weeks.

[0389] △: No increase in precipitates was observed after 4 days, but an increase in precipitates was observed after 1 week.

[0390] ×: An increase in precipitates was observed after 1 day.

[0391] <Acid resistance>

[0392] The solid pattern thus prepared was immersed in a 10% HCl aqueous solution at 25° C. for 30 minutes, and then washed with pure water. The water was wiped off and the same evaluation as the above-mentioned adhesion was performed.

[0393] (Benchmark)

[0394] ◎: The adhesion remaining rate is 100%.

[0395] ○: The adhesion residual rate is 80% or more and less than 100%.

[0396] △: The adhesion residual rate is 60% or more and less than 80%.

[0397] ×: The adhesion residual rate is less than 60%.

[0398] <Alkali resistance>

[0399] The solid pattern thus prepared was immersed in a 10% NaOH aqueous solution at 25° C. for 30 minutes, and then washed with pure water. The water was wiped off and the same evaluation as the above-mentioned adhesion was performed.

[0400] (Benchmark)

[0401] ◎: The adhesion remaining rate is 100%.

[0402] ○: The adhesion residual rate is 80% or more and less than 100%. △: The adhesion residual rate is 60% or more and less than 80%. ×: The adhesion residual rate is less than 60%.

[0403]

[0404] As shown in the above results, the ink of the present invention has higher adhesion and can obtain sufficient hardness than the ink of the comparative example, and can suppress the increase in viscosity during long-term storage and retention, and can suppress the change in particle size and the generation of precipitates.

[0405] In the case of ink 9 using caprolactam-modified dipentaerythritol hexaacrylate, in particular, the acid resistance and alkali resistance were excellent.

Claims

1. An inkjet ink composition which is a composition curable by active energy rays or heat, in, The inkjet ink composition comprises: A compound having a structure represented by the following general formula (1) or a salt thereof (A); and Hyperbranched acrylate oligomer or polymer (B), The content of the compound having a structure represented by the following general formula (1) or its salt (A) is in the range of 1 to 50% by mass relative to the total ink; the content of the hyperbranched acrylate oligomer or polymer (B) is in the range of 5 to 50% by mass relative to the total ink, [Chemical formula 1] General formula (1) In the general formula (1), X represents a substituent having at least one selected from acryloyl, methacryloyl, allyl, vinyl and derivatives thereof at the terminal. Q represents an oxygen atom or NR 4 , R 4 represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, R 1 It represents an unsubstituted alkylene group having 1 to 6 carbon atoms.

2. The inkjet ink composition according to claim 1, in, In the general formula (1), X represents an acryloyl group or a methacryloyl group.

3. The inkjet ink composition according to claim 1 or 2, in, In the general formula (1), Q represents an oxygen atom.

4. The inkjet ink composition according to claim 1 or 2, in, In the general formula (1), R 1 It represents an unsubstituted alkylene group having 1 or 2 carbon atoms.

5. The inkjet ink composition according to claim 1 or 2, further comprising: A polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B).

6. The inkjet ink composition according to claim 5, in, The polyfunctional (meth)acrylate (C) having three or more (meth)acryloyl groups other than the hyperbranched acrylate oligomer or polymer (B) is caprolactam-modified dipentaerythritol hexaacrylate.

7. The inkjet ink composition according to claim 1 or 2, further comprising: A (meth)acrylate compound (D) having a ClogP value within a range of 4.0 to 7.

0.

8. The inkjet ink composition according to claim 1 or 2, further comprising: Gelling agent (E). 9 . The inkjet ink composition according to claim 1 or 2 , which is used as an inkjet ink for forming a solder resist pattern used in a printed circuit board. 10 . A recorded matter obtained by curing the inkjet ink composition according to claim 1 with active energy rays or heat.

11. An inkjet recording method, which is an inkjet recording method using an inkjet ink composition, in, Using the inkjet ink composition according to any one of claims 1 to 9, and The inkjet recording method has: A step of ejecting the inkjet ink composition from an inkjet head to drop onto a recording medium; and A step of curing the inkjet ink composition that has landed on a recording medium by active energy rays or heat.

12. An inkjet recording system, which is an inkjet recording system using an inkjet ink composition, in, Using the inkjet ink composition according to any one of claims 1 to 9, and The inkjet recording system has: An inkjet head for ejecting the inkjet ink composition, an active energy ray irradiation unit for irradiating the inkjet ink composition landed on a recording medium with active energy rays, and a heating unit for heating the inkjet ink composition irradiated with the active energy rays.

Citation Information

Patent Citations

  • Foam wallpaper original fabric and foam wallpaper

    JP2018178468A

  • Inkjet ink for resist

    JP2020037645A

  • Inkjet ink and method for producing printed matter using the inkjet ink

    JP2018062585A

Cited By

  • Ink jet for coiled material pipe in high-temperature and high-humidity environment, coiled material pipe ink jet method and coiled material pipe

    CN119505600A