A porous functional coated membrane and its preparation method, and a lithium-ion battery

By using a composite material of PMMA, lithium oxalate, and porous carbon to form a porous functional coating on the lithium-ion battery separator, the problems of increased air permeability during PVDF coating and pore collapse during hot pressing are solved, thereby improving battery performance.

CN116780097BActive Publication Date: 2026-11-10安徽得壹能源科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310850028.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-11
Publication Date
2026-11-10
Estimated Expiration
2043-07-11

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators have the problem of increased air permeability during the PVDF coating process, and the porous structure is prone to collapse during hot pressing, which affects battery performance.

Method used

A porous functional coating is formed by using PMMA, lithium oxalate and porous carbon composite materials. Lithium salt is provided by the decomposition of lithium oxalate during hot pressing, which improves adhesion and reduces decomposition voltage, avoids pore blockage, and utilizes porous carbon to provide effective lithium ion channels.

Benefits of technology

It improves the first-cycle coulombic efficiency and cycle performance of lithium-ion batteries, enhances the liquid retention capacity and ion permeability of the separator, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116780097B_ABST
    Figure CN116780097B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of battery technology, specifically relating to lithium-ion battery separators, and more specifically to a porous functional coating separator, its preparation method, and a lithium-ion battery. The porous functional coating separator includes a separator base layer and a porous functional coating. The porous functional coating is located on one side of the separator base layer and is formed by mixing PMMA with a lithium-replenishing composite material. The lithium-replenishing composite material is a composite of lithium oxalate and porous carbon, with the lithium oxalate filling the pore structure of the porous carbon and / or coating the surface of the porous carbon. When using this separator to prepare a lithium-ion battery, during hot pressing, the porous functional coating bonds the separator to the positive electrode. During formation, the lithium oxalate in the lithium-replenishing composite material decomposes into lithium salt and carbon dioxide. This invention can improve the ion transmission efficiency of the separator after hot pressing and enhance the lithium-replenishing function of the adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, and relates to lithium-ion battery separators, specifically to a porous functional coating separator and its preparation method, and a lithium-ion battery. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] As one of the four main materials of lithium-ion batteries, the separator plays a crucial role in preventing short circuits between the positive and negative electrodes. Simultaneously, its microporous structure provides effective channels for ions, forming a complete charge-discharge circuit. Currently, commercially used separator materials are primarily polyethylene (PE) and polypropylene (PP), coated with ceramic or high-temperature resistant organic materials to enhance high-temperature resistance. To improve cell hardness and the interface between the separator and the electrodes, an adhesive layer is typically added. Common coating methods primarily involve aqueous / oil-based coatings of polyvinylidene fluoride (PVDF), but these methods suffer from increased permeability and pore blockage, leading to increased internal resistance. Furthermore, during the initial charge-discharge process, the formation of the SEI film consumes some active lithium ions, resulting in lower initial charge-discharge efficiency and a decrease in battery capacity and energy density.

[0004] The industry typically addresses the increased permeability during the oil-based PVDF coating process by creating pores or by using spraying for localized coating to reduce the increase in permeability. However, the inventors' research has revealed the following problems with current pore-forming processes used to improve the increased permeability during oil-based PVDF coating: 1. Adding a pore-forming agent requires extraction and curing before pore formation, a cumbersome and costly process; 2. The pore-formed PVDF-coated separator is prone to collapse during the hot-pressing process of the battery cell, leading to increased permeability and affecting the battery's rate performance. Summary of the Invention

[0005] In order to improve the ion passage efficiency of the separator after hot pressing and to enable the lithium replenishment function of the adhesive layer, the present invention aims to provide a porous functional coating separator and its preparation method, and a lithium-ion battery.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows: On one hand, a porous functional coating membrane includes a membrane base layer and a porous functional coating, wherein the porous functional coating is located on one side of the membrane base layer, and the porous functional coating is formed by mixing PMMA (polymethyl methacrylate) with a lithium-supplementing composite material, wherein the lithium-supplementing composite material is a composite material of lithium oxalate and porous carbon, and the lithium oxalate is filled in the pore structure of the porous carbon, and / or the lithium oxalate is coated on the surface of the porous carbon; When preparing a lithium-ion battery using the aforementioned separator, during the hot pressing process, the porous functional coating bonds the separator to the positive electrode sheet; during the formation process, lithium oxalate in the lithium-replenishing composite material decomposes into lithium salt and carbon dioxide.

[0007] To avoid pore collapse and blockage during hot pressing, this invention employs a binder and porous materials. By pre-composite a lithium replenishing agent to the porous material, not only is pore blockage by the binder avoided during hot pressing, but lithium replenishment and energization of the porous functional coating are also achieved. Lithium oxalate is chosen as the lithium replenishing agent because it decomposes during the formation process, thus opening up the pores in the porous material. Porous carbon is selected to reduce the decomposition voltage of lithium oxalate during formation, effectively improving battery performance. However, when using conventional PVDF binders, the addition of lithium replenishing composite materials significantly reduces the adhesion between the porous functional coating and the electrode, which is detrimental to the bonding between the separator and the electrode. Therefore, this invention selects PMMA as the binder, as the adhesion between the porous functional coating formed by PMMA and the lithium replenishing composite material does not significantly decrease, and is more conducive to the bonding between the separator and the electrode, thereby ensuring the cell's hardness and interface performance.

[0008] On the other hand, a method for preparing the above-mentioned porous functional coating membrane includes the following steps: Lithium-supplemented composite materials are obtained by filling the porous carbon pore structure with lithium oxalate through recrystallization and / or coating the surface of porous carbon with lithium oxalate. PMMA is dispersed in an organic solvent to obtain a PMMA slurry; The lithium-supplemented composite material is added to PMMA slurry and dispersed evenly to obtain a composite slurry. The composite slurry is then roller-coated onto one side of the membrane substrate to form a porous functional coating.

[0009] Thirdly, a lithium-ion battery, wherein the lithium-ion battery is a hot-pressed composite cell, comprising a positive electrode, the aforementioned porous functional coating separator, an electrolyte, and a negative electrode, wherein the positive electrode, the porous functional coating separator, and the negative electrode are formed by hot-pressing composite.

[0010] The beneficial effects of this invention are as follows: Compared to traditional lithium replenishing agents, this invention selects lithium oxalate, which is easy to store and use. When combined with porous carbon (especially ordered mesoporous carbon), lithium oxalate decomposes into lithium salt and carbon dioxide during the formation stage. The lithium salt participates in the battery's lithium-ion cycle as a lithium replenishing agent, while the generated carbon dioxide gas is discharged during the formation stage. Simultaneously, the addition of porous carbon effectively reduces the decomposition voltage of lithium oxalate. Battery cells (lithium-ion batteries) made using the porous functional coating separator provided by this invention show significant improvements in first-cycle coulombic efficiency and cycle performance. A higher first-cycle coulombic efficiency indicates a better lithium replenishment effect. The replenished lithium source is used for the formation of the SEI film, increasing the utilization rate of active lithium in the cathode material and extending cycle life. Furthermore, since the lithium oxalate in the ordered mesoporous carbon has already decomposed and entered the battery cycle, the vacated channels provide lithium-ion shuttles, acting as a pore-forming agent, reducing the separator's permeability, and thus improving the separator's liquid retention capacity and ion permeability. Attached Figure Description

[0011] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0012] Figure 1 This is a SEM image of the ordered mesoporous carbon CMK-3 used in the embodiments of the present invention; Figure 2 The diagram shows the structure of the porous functional coating membrane prepared according to an embodiment of the present invention: 1. Lithium-supplemented composite material, 2. PMMA binder, 3. Membrane base layer. Detailed Implementation

[0013] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0014] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0015] Given that existing methods for improving air permeability through pore formation in separators are not suitable for hot-pressed composite cells and that the formation of SEI during the first charge and discharge of lithium-ion batteries consumes some active lithium ions, this invention proposes a porous functional coating separator, its preparation method, and a lithium-ion battery.

[0016] A typical embodiment of the present invention provides a porous functional coating membrane, comprising a membrane base layer and a porous functional coating, wherein the porous functional coating is located on one side of the membrane base layer, and the porous functional coating is formed by mixing PMMA with a lithium-supplementing composite material, wherein the lithium-supplementing composite material is a composite material of lithium oxalate and porous carbon, and the lithium oxalate fills the pore structure of the porous carbon, and / or the lithium oxalate is coated on the surface of the porous carbon. When preparing a lithium-ion battery using the aforementioned separator, during the hot pressing process, the porous functional coating bonds the separator to the positive electrode sheet; during the formation process, lithium oxalate in the lithium-replenishing composite material decomposes into lithium salt and carbon dioxide.

[0017] During hot pressing, PMMA bonds the separator to the electrode, ensuring the cell's rigidity and interface performance. During formation, lithium oxalate in the ordered mesoporous carbon decomposes into lithium salt and carbon dioxide; the carbon dioxide is removed during the venting process, while the lithium salt dissolves in the electrolyte and participates in battery cycling. The resulting open channels in the mesoporous carbon provide space for lithium ions to shuttle, thereby improving the separator's electrolyte retention and ion permeability.

[0018] By co-coating PMMA with lithium-added composite materials, the pores of the ordered mesoporous carbon are less likely to be blocked by PMMA during hot pressing due to the filling of lithium oxalate. During formation, lithium oxalate decomposes, allowing ions to pass through the pores. Compared to traditional binder layers, its pore structure is formed after the hot pressing process of the battery cell, avoiding collapse during hot pressing. Therefore, it has a higher porosity and provides lithium-added energy to the binder layer.

[0019] In some embodiments, the porous carbon is one or more selected from ordered mesoporous carbon CMK-3, nanoporous carbon NCP, porous activated carbon, porous carbon nanotubes, porous carbon fibers, and porous carbon aerogels. Ordered mesoporous carbon CMK-3 is preferred.

[0020] In some embodiments, the mass ratio of PMMA to lithium-added composite material is 8~10:2~5.

[0021] In some embodiments, the diaphragm base layer is a diaphragm substrate or a ceramic composite diaphragm. The diaphragm substrate is made of PP or PE. The ceramic composite diaphragm is made of a polymer-ceramic composite material, wherein the polymer is PP or PE.

[0022] Another embodiment of the present invention provides a method for preparing the above-mentioned porous functional coating membrane, comprising the following steps: Lithium-supplemented composite materials are obtained by filling the porous carbon pore structure with lithium oxalate through recrystallization and / or coating the surface of porous carbon with lithium oxalate. PMMA is dispersed in an organic solvent to obtain a PMMA slurry; The lithium-supplemented composite material is added to PMMA slurry and dispersed evenly to obtain a composite slurry. The composite slurry is then roller-coated onto one side of the membrane substrate to form a porous functional coating.

[0023] In some embodiments, the process of preparing the lithium-replenishing composite material by recrystallization is as follows: water is heated to 80-100°C, lithium oxalate is added to prepare a saturated solution, porous carbon is added and dispersed evenly, the temperature is lowered to 0-50°C, and the mixture is filtered to obtain the lithium-replenishing composite material. After adding the porous carbon, the stirring speed for even dispersion is 500-1000 r / min, and the stirring time is 10-40 min.

[0024] In one or more embodiments, the mass ratio of water, lithium oxalate, and porous carbon is 80~100:2~8:5~15.

[0025] In some embodiments, N-methylpyrrolidone is used as the organic solvent in preparing PMMA slurry.

[0026] In some embodiments, a planetary mixer is used to prepare the PMMA slurry. The mixing time is 60-90 min, and the mixing speed is 30-40 r / min for revolution and 800-1500 r / min for rotation.

[0027] In some embodiments, when preparing PMMA slurry, the PMMA particle size is 0.2~10μm.

[0028] In some embodiments, the lithium-added composite material is added to the PMMA slurry and stirred using a planetary mixer to ensure uniform dispersion. The stirring time is 60-90 min, and the stirring speed is 30-40 r / min for revolution and 800-1500 r / min for rotation.

[0029] In some embodiments, the composite paste is applied to one side of the diaphragm substrate using a gravure roller. The coating thickness is preferably 1–10 μm. The coating speed is preferably 20–100 m / min. The gravure roller speed ratio is preferably 50–120%. The oven temperature is preferably 50–100 °C. The unwinding tension is preferably 10–30 N. The oven tension is preferably 10–35 N. The winding tension is preferably 10–30 N.

[0030] A third embodiment of the present invention provides a lithium-ion battery, wherein the lithium-ion battery is a hot-pressed composite cell, comprising a positive electrode, the aforementioned porous functional coating separator, an electrolyte, and a negative electrode, wherein the positive electrode, the porous functional coating separator, and the negative electrode are formed by hot-pressing composite.

[0031] Specifically, the positive electrode sheet is composed of a positive electrode material, a binder, a conductive agent, and a current collector. The positive electrode material of the positive electrode sheet can be lithium nickel cobalt manganese oxide.

[0032] Specifically, the negative electrode sheet is composed of a negative electrode material, a binder, a conductive agent, and a current collector. The negative electrode material of the negative electrode sheet can be graphite.

[0033] Specifically, the preparation process of lithium-ion batteries includes a hot pressing process, wherein the hot pressing temperature is 50~100℃, the hot pressing time is 20~180s, and the hot pressing pressure is 0.1~0.6MPa.

[0034] Specifically, the preparation process of lithium-ion batteries includes a formation process, wherein the charging current is 0.01~0.33C, the cutoff voltage is 3.7~4.5V, the formation pressure is 0.1~0.8MPa, and the formation temperature is 30~70℃.

[0035] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments and comparative examples.

[0036] Example 1 The preparation method of the porous functional coated membrane includes the following steps: 1. Preparation of lithium-added composite material: Heat 100 kg of deionized water to 90°C, add 3 kg of lithium oxalate to prepare a saturated solution, and add 5 kg of ordered mesoporous carbon CMK-3 (surface structure as shown in the figure). Figure 1 (As shown) The mixture was dispersed and stirred using a high-speed mixer for 30 minutes at a speed of 800 r / min. It was then cooled to 25°C, recrystallized, and filtered to obtain the lithium-replenishing composite material.

[0037] 2. PMMA slurry preparation: Dissolve 10 kg PMMA in 100 kg N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PMMA particle size is 0.8 μm.

[0038] 3. Preparation of composite slurry: Add 5 kg of lithium-supplemented composite material from step 1 to the PMMA solution obtained in step 2, and mix them using a planetary mixer for 75 min. The stirring speed is 35 r / min for revolution and 1200 r / min for rotation.

[0039] 4. Apply the composite slurry from step 3 to one side of the 9μm PE substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0040] The structure of the porous functional coated membrane is prepared as follows: Figure 2As shown, a porous functional coating is formed on the surface of the membrane base layer 3. The porous functional coating is formed by wrapping and bonding PMMA binder 2 onto the lithium-supplementing composite material 1.

[0041] Example 2 The preparation method of the porous functional coated membrane includes the following steps: 1. Preparation of lithium-replenishing composite material: 100 kg of deionized water was heated to 90 °C, 3 kg of lithium oxalate was added to prepare a saturated solution, 5 kg of ordered mesoporous carbon CMK-3 was added and dispersed and stirred by a high-speed stirrer for 30 min at a stirring speed of 800 r / min, cooled to 45 °C for recrystallization and filtered to obtain the lithium-replenishing composite material.

[0042] 2. PMMA slurry preparation: Dissolve 10 kg PMMA in 100 kg N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PMMA particle size is 0.8 μm.

[0043] 3. Preparation of composite slurry: Add 5 kg of lithium-supplemented composite material from step 1 to the PMMA solution obtained in step 2, and mix them using a planetary mixer for 75 min. The stirring speed is 35 r / min for revolution and 1200 r / min for rotation.

[0044] 4. Apply the composite slurry from step 3 to one side of the substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0045] Example 3 The preparation method of the porous functional coated membrane includes the following steps: 1. Preparation of lithium-replenishing composite material: 100 kg of deionized water was heated to 90 °C, 3 kg of lithium oxalate was added to prepare a saturated solution, 5 kg of ordered mesoporous carbon CMK-3 was added and dispersed and stirred by a high-speed stirrer for 30 min at a stirring speed of 800 r / min, cooled to 60 °C for recrystallization and filtered to obtain the lithium-replenishing composite material.

[0046] 2. PMMA slurry preparation: Dissolve 10 kg PMMA in 100 kg N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PMMA particle size is 0.8 μm.

[0047] 3. Preparation of composite slurry: Add 5 kg of lithium-supplemented composite material from step 1 to the PMMA solution obtained in step 2, and mix them using a planetary mixer for 75 min. The stirring speed is 35 r / min for revolution and 1200 r / min for rotation.

[0048] 4. Apply the composite slurry from step 3 to one side of the substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0049] Example 4 The preparation method of the porous functional coated membrane includes the following steps: 1. Preparation of lithium-replenishing composite material: 100 kg of deionized water was heated to 90 °C, 3 kg of lithium oxalate was added to prepare a saturated solution, 5 kg of ordered mesoporous carbon CMK-3 was added and dispersed and stirred by a high-speed stirrer for 30 min at a stirring speed of 800 r / min, cooled to 45 °C for recrystallization and filtered to obtain the lithium-replenishing composite material. 2. PMMA slurry preparation: Dissolve 7 kg of PMMA in 100 kg of N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PMMA particle size is 0.8 μm. 3. Preparation of composite slurry: Add 5 kg of lithium-supplemented composite material from step 1 to the PMMA solution obtained in step 2, and mix them using a planetary mixer for 75 min. The stirring speed is 35 r / min for revolution and 1200 r / min for rotation.

[0050] 4. Apply the composite slurry from step 3 to one side of the substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0051] Comparative Example 1 The preparation method of the porous functional coated membrane includes the following steps: 1. Preparation of lithium-replenishing composite material: 100 kg of deionized water was heated to 90 °C, 3 kg of lithium oxalate was added to prepare a saturated solution, 5 kg of ordered mesoporous carbon CMK-3 was added and dispersed and stirred by a high-speed stirrer for 30 min at a stirring speed of 800 r / min, cooled to 45 °C for recrystallization and filtered to obtain the lithium-replenishing composite material.

[0052] 2. PVDF slurry preparation: Dissolve 10 kg of PVDF in 100 kg of N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PVDF particle size is 0.8 μm.

[0053] 3. Preparation of composite slurry: Add 5 kg of lithium-supplemented composite material from step 1 to the PVDF solution obtained in step 2, and mix them using a planetary mixer for 75 min. The stirring speed is 35 r / min for revolution and 1200 r / min for rotation.

[0054] 4. Apply the composite slurry from step 3 to one side of the substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0055] Comparative Example 2 The preparation method of the diaphragm is as follows: 1. PMMA slurry preparation: Dissolve 10 kg PMMA in 100 kg N-methylpyrrolidone and stir thoroughly using a planetary mixer for 60 min. The stirring speed is 30 r / min for revolution and 800 r / min for rotation. The PMMA particle size is 0.8 μm.

[0056] 2. Apply the PMMA slurry from step 1 to one side of the substrate diaphragm using a gravure roller. The coating thickness is 2μm. The coating speed is 50m / min, the gravure roller speed ratio is 80%, the oven temperature is 80℃, the unwinding tension is 20N, the oven tension is 18N, and the rewinding tension is 15N.

[0057] Battery fabrication: Lithium nickel cobalt manganese oxide, PVDF binder, CNT, and SP conductive agent were mixed with NMP solvent at a mass ratio of 96:2:1:1 and stirred for 6 hours. The mixture was then coated onto aluminum foil using a coating machine, dried, rolled, and slit to obtain the positive electrode sheet. Graphite, aqueous binder, CNT, and SP were mixed with solvent at a mass ratio of 94:4:0.5:0.5:1. The slurry was then coated onto copper foil, dried, rolled, and slit to obtain the negative electrode sheet. The electrolyte was 1 mol / L LiPF6 / EC+PC+DEC+EMC (volume ratio 1:0.3:1:1). The above positive and negative electrode sheets, along with the separators from the examples and comparative examples, were used to fabricate a pouch battery.

[0058] Hot pressing process: The prepared battery cells are hot pressed using a hot press at a temperature of 80℃ for 120 seconds and a pressure of 0.3MPa.

[0059] Formation process: The hot-pressed battery cells are placed on the formation cabinet for charging. The charging current is 0.1C, the cut-off voltage is 4.3V, the formation pressure is 0.6MPa, and the formation temperature is 45℃.

[0060] After formation, the battery undergoes gas bag removal and secondary sealing.

[0061] The physical properties of the separators in Examples 1-4 and Comparative Examples 1-2, as well as the electrochemical performance of the pouch cells, were tested using the following methods: Physical property testing: Air permeability testing was performed using an Asahi EG01-55-1MR instrument from Japan. The diaphragm to be tested was cut into 10×10cm samples for testing. Adhesion testing was performed using a universal tensile testing machine. During the test, the diaphragm to be tested was hot-pressed to the electrode at a temperature of 80℃ for 60 seconds. After hot pressing, the sample was fixed on the tensile testing machine for a 180° tensile adhesion test. Electrical performance testing: The battery is charged and discharged using a charge and discharge tester. The charge and discharge capacity data is tested under 0.33C conditions, and the cycle performance test is repeated.

[0062] The test results are shown in Tables 1 and 2.

[0063] Table 1. Comparison of physical properties of the diaphragms in Examples 1-4 and Comparative Examples 1-2

[0064] By comparing the various embodiments and Comparative Example 1 in Table 1, the electrode adhesion was significantly improved, but decreased somewhat compared to Comparative Example 2. This indicates that PMMA has higher electrode adhesion than PVDF coating, and no significant decreasing trend was observed compared to continuous phase PMMA adhesion. In the embodiments, the cell separator after the first cycle was tested, and the air permeability decreased significantly, while in Example 2 it increased significantly. This proves that lithium oxalate has decomposed and entered the cycle, and its ordered mesoporous carbon channel structure provides an effective channel for ion transport. In the embodiments, part of the PMMA adhesive layer entered the separator pores, causing pore blockage and a sharp increase in air permeability. This shows that the hot-pressing formation pore-forming method of the present invention is conducive to the formation of ion channels, thereby reducing the air permeability of the separator.

[0065] Table 2 Electrochemical performance of pouch cells using the separators of Examples 1-4 and Comparative Examples 1-2

[0066] As shown in Table 2, the lithium-replenishing material cells in the embodiments exhibit significant improvements in both first-cycle coulombic efficiency and cycle performance. Higher first-cycle coulombic efficiency indicates better lithium replenishment, with the replenished lithium source used for SEI film formation. This increases the utilization rate of active lithium in the cathode material and extends cycle life. Furthermore, it demonstrates that lithium oxalate in the ordered mesoporous carbon has decomposed and entered the battery cycle, with the vacated channels providing lithium-ion shuttles, thus playing a role in both pore formation and lithium replenishment.

[0067] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A porous functional coated membrane, characterized in that, The membrane includes a diaphragm base layer and a porous functional coating. The porous functional coating is located on one side of the diaphragm base layer and is formed by mixing PMMA with a lithium-supplementing composite material. The lithium-supplementing composite material is a composite material of lithium oxalate and porous carbon, and the lithium oxalate is filled in the pore structure of the porous carbon and / or the lithium oxalate is coated on the surface of the porous carbon. When the separator is used to prepare a lithium-ion battery, during the hot pressing process, the porous functional coating bonds the separator to the positive electrode sheet; during the formation process, lithium oxalate in the lithium-replenishing composite material decomposes into lithium salt and carbon dioxide. Its preparation method includes the following steps: Lithium-supplemented composite materials are obtained by filling the porous carbon pore structure with lithium oxalate through recrystallization and / or coating the surface of porous carbon with lithium oxalate. PMMA is dispersed in an organic solvent to obtain a PMMA slurry; The lithium-supplemented composite material is added to PMMA slurry and dispersed evenly to obtain a composite slurry. The composite slurry is then roller-coated onto one side surface of the membrane substrate to form a porous functional coating. The process of preparing lithium-replenishing composite material by recrystallization is as follows: water is heated to 80~100 ℃, lithium oxalate is added to prepare a saturated solution, porous carbon is added and dispersed evenly, the temperature is lowered to 0~50 ℃, and the solution is filtered to obtain lithium-replenishing composite material.

2. The porous functional coating membrane as described in claim 1, characterized in that, The porous carbon is one or more of ordered mesoporous carbon CMK-3, nanoporous carbon NCP, porous activated carbon, porous carbon nanotubes, porous carbon fibers, and porous carbon aerogels.

3. The porous functional coating membrane as described in claim 1, characterized in that, The mass ratio of PMMA to lithium-added composite material is 8~10:2~5.

4. The porous functional coating membrane as described in claim 1, characterized in that, The organic solvent used in the preparation of PMMA slurry is N-methylpyrrolidone; Alternatively, when preparing PMMA slurry, the PMMA particle size is between 0.2 and 10 μm.

5. The porous functional coating membrane as described in claim 1, characterized in that, The mass ratio of water, lithium oxalate, and porous carbon is 80~100:2~8:5~15.

6. The porous functional coating membrane as described in claim 1, characterized in that, The lithium-added composite material was added to the PMMA slurry and stirred using a planetary mixer to ensure uniform dispersion.

7. The porous functional coating membrane as described in claim 6, characterized in that, The stirring time is 60~90min, and the stirring speed is 30~40r / min for revolution and 800~1500r / min for rotation.

8. The porous functional coating membrane as described in claim 1, characterized in that, The composite slurry is applied to one side of the diaphragm base layer using a gravure roller.

9. The porous functional coated diaphragm as described in claim 8, characterized in that, The coating thickness is 1~10μm.

10. The porous functional coated diaphragm as described in claim 8, characterized in that, The coating speed is 20~100m / min.

11. The porous functional coated diaphragm as described in claim 8, characterized in that, The gravure roller speed ratio is 50~120%.

12. The porous functional coated diaphragm as described in claim 8, characterized in that, The oven temperature is 50~100℃.

13. The porous functional coated diaphragm as described in claim 8, characterized in that, The unwinding tension is 10~30N.

14. The porous functional coating membrane as described in claim 8, characterized in that, The oven tension is 10~35N.

15. The porous functional coated diaphragm as described in claim 8, characterized in that, The winding tension is 10~30N.

16. A lithium-ion battery, characterized in that, The lithium-ion battery cell is a hot-pressed composite cell, comprising a positive electrode, a porous functional coating separator as described in any one of claims 1 to 15, an electrolyte, and a negative electrode, wherein the positive electrode, the porous functional coating separator, and the negative electrode are formed by hot-pressing composite.

17. The lithium-ion battery as described in claim 16, characterized in that, The positive electrode material of the positive electrode sheet is lithium nickel cobalt manganese oxide; Alternatively, the negative electrode material of the negative electrode sheet is graphite; Alternatively, the lithium-ion battery manufacturing process includes a hot-pressing process, wherein the hot-pressing temperature is 50~100℃, the hot-pressing time is 20~180s, and the hot-pressing pressure is 0.1~0.6MPa. Alternatively, the lithium-ion battery preparation process includes a formation process, wherein the charging current is 0.01~0.33C, the cutoff voltage is 3.7~4.5V, the formation pressure is 0.1~0.8MPa, and the formation temperature is 30~70℃.

Citation Information

Patent Citations

  • Lithium supplementing composite diaphragm and preparation method thereof

    CN112271405A

  • Nondestructive lithium-supplementing composite diaphragm as well as preparation method and application thereof

    CN114552125A