A composite self-healing anti-corrosion coating material and preparation method thereof
By introducing polyacrylate elastomer and metal salt into the self-healing coating material, combined with gas phase nanomaterials and silicon nanomaterials, a composite self-healing anti-corrosion coating is prepared, which solves the problem of existing self-healing coating materials in high anti-corrosion environments. It achieves efficient self-healing and durability improvement by solving the problem of limited application in China.
Patent Information
- Application Number
- CN202310970214.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-08-03
AI Technical Summary
Existing self-healing coating materials have limited application in environments with high anti-corrosion requirements. The self-healing behavior is not completely spontaneous and requires manual fixation of damage. The durability performance is insufficient, including defects in adhesion strength, impedance and water resistance.
A composite self-healing anti-corrosion coating material is used, including a base layer, a paint layer, a self-healing elastomer layer and a super-hydrophobic polyurethane layer. The self-healing elastomer layer is composed of polyacrylate elastomer and metal salt and is prepared by spraying. , introducing gas phase nanomaterials and silicon nanomaterials to improve the corrosion resistance and self-healing capabilities of the coating.
It achieves rapid self-healing in high-salt and high-humidity environments, improves the durability and self-healing ability of the coating, enhances adhesion and resistance, and extends the service life of the coating.
Smart Images

Figure CN116786384B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of self-repairing anti-corrosion coating materials, and in particular to the technical field of preparing self-repairing polyacrylate anti-corrosion coating materials. Background Art
[0002] Metal corrosion is a serious problem faced by metals and alloy materials in practical applications, which can cause serious safety hazards, economic losses and environmental pollution. The use of organic coating materials is one of the most effective ways to inhibit metal corrosion. Organic coatings can act as physical barriers to isolate metals from corrosive ions, oxygen and water, and play a special role in corrosion prevention. However, in long-term contact with corrosive media, moisture on the surface of the organic coating will inevitably penetrate into the coating, weakening the isolation effect of the coating and causing metal corrosion. To solve this problem, self-healing coating materials have become a new hot research direction for metal corrosion protection. Self-healing coating materials can self-repair after the coating is damaged, restore the material's corrosion resistance, and improve the material's long-term corrosion resistance.
[0003] According to the different protection mechanisms, self-healing coating materials include external healing protective coatings and internal healing protective coatings. In external healing protective coating materials, microcapsules, fiber tubes, inorganic nanoparticles, etc. are wrapped by repair agents and dispersed in the coating substrate. When the anti-corrosion environment is damaged, the repair agent is released to inhibit corrosion reactions or repair coating defects. Its repair effect is irreversible, and the content of the repair agent is limited by the material, so the self-repair efficiency is low and the economic cost is high. The internal healing protective coating mainly achieves self-repair through the molecular action of the material itself, and can repair the damage of the material through the reversible fracture and recombination characteristics between dynamic bonds, and restore the inherent function and structure of the material under external stimulation.
[0004] Although intrinsic healing protective coatings, namely intrinsic self-healing coating materials, have made great progress, there are still many problems, including: the self-healing behavior of most existing self-healing coating materials is not completely spontaneous, and they need to be manually fixed when the damage just occurs; most existing self-healing coating materials can only self-repair in the air; most existing self-healing coating materials generally sacrifice durability, including adhesion strength, long-term impedance and long-term water resistance, which obviously limit the wide application of materials in fields with complex anti-corrosion requirements. Summary of the invention
[0005] In view of the defects of the prior art, the object of the present invention is to provide a composite anti-corrosion coating material and a preparation method thereof which has high durability, can heal spontaneously and rapidly, has excellent self-healing ability, and can be stably used in environments with high anti-corrosion requirements.
[0006] The technical solution of the present invention is as follows:
[0007] A composite self-healing anti-corrosion coating material, which comprises in sequence: a base layer, a paint layer, a self-healing elastomer layer and a super-hydrophobic polyurethane layer, wherein the self-healing elastomer layer comprises a polyacrylate elastomer and a metal salt having the following structure:
[0008]
[0009] in:
[0010] R1 is selected from any one of the following structures:
[0011]
[0012] R2 is selected from any one of the following structures:
[0013]
[0014] R3 is selected from any one of the following structures:
[0015]
[0016] R4 is selected from any one of the following structures:
[0017]
[0018] R5 is selected from any one of the following structures:
[0019]
[0020] and:
[0021] a: b: c: d=100: (15-30): (0.5-8): (0.5-4);
[0022] Wherein, the super-hydrophobic polyurethane layer comprises a polyurethane material with super-hydrophobic material distributed on the surface.
[0023] Preferably, the self-healing elastic elastomer layer further comprises gas phase nanomaterials and / or silicon nanomaterials.
[0024] Further preferably, the gas-phase nanomaterial is selected from gas-phase hydrophobic silica and / or gas-phase white carbon black.
[0025] Preferably, the super-hydrophobic polyurethane layer comprises a polyurethane material having a super-hydrophobic material distributed on the surface, and the super-hydrophobic material is selected from one or more of precipitated calcium carbonate, carbon nanotubes, and silicon nanomaterials.
[0026] Preferably, the super hydrophobic material is distributed in an epoxy resin system, and the epoxy resin system is fixed on the surface of the polyurethane material.
[0027] Preferably, the base layer is formed of a carbon steel sheet.
[0028] Preferably, the paint layer comprises a zinc-rich primer.
[0029] Preferably, the self-healing elastomer layer in the composite self-healing anti-corrosion coating material is prepared by a preparation method comprising the following processes:
[0030] The raw material components A, B, C, D and E of the polyacrylate elastomer are mixed, reacted at 65-75° C., and then allowed to stand to obtain a transparent reaction solution, the obtained reaction solution is precipitated with petroleum ether, the obtained precipitate is vacuum dried and dissolved in an organic solvent, and then a dispersion of gas-phase nanomaterials and / or silicon nanomaterials and an organic solution of metal salts are added, mixed evenly, added to a mold, and cured at 65-75° C. to obtain the self-healing elastomer layer;
[0031] Wherein, the component A is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, and isooctyl acrylate; the component B is selected from one or more of acrylonitrile, acrylic acid, benzyl methacrylate, and 2-methyl-2-acrylic acid-2-(2-methoxyethoxy)ethyl ester; the component C is selected from 1,4-dioxane and / or tetrahydrofuran; the component D is selected from one or more of 4-vinylpyridine, 4-vinylimidazole, divinylbenzene, and n-dodecyl mercaptan; the component E is selected from 2,2'-azobisisobutyronitrile and / or dibenzoyl peroxide; and the mass ratio of the component A to the component B is 1:0.1 to 0.5.
[0032] Preferably, the raw material of the polyacrylate elastomer further includes component F, and the component F is selected from silane coupling agents such as KH570, KH580 and the like.
[0033] Preferably, the metal salt is selected from one or more of cobalt chloride, copper chloride, zinc chloride, ferric chloride, and lithium bis(difluorosulfonyl)imide.
[0034] The present invention further provides a method for integrally preparing the composite self-healing anti-corrosion coating material, which comprises the following steps:
[0035] (1) forming a semi-cured paint layer on the base layer by spraying to obtain a first semi-cured coating base;
[0036] (2) mixing the raw material components of the polyacrylate elastomer, reacting them at 65-75° C., and then standing to obtain a transparent reaction solution, precipitating the obtained reaction solution with petroleum ether, vacuum drying the obtained precipitate, and then dissolving it in an organic solvent to obtain a first dissolved solution;
[0037] (3) adding metal salt and / or organic solution of metal salt and organic solution of gas phase nanomaterial and / or silicon nanomaterial to the first dissolved substance solution to obtain a second coating solution;
[0038] (4) spraying the second coating solution onto the first semi-cured coating substrate and semi-curing at room temperature to obtain a second semi-cured coating substrate;
[0039] (5) mixing the polyurethane coating and the curing agent uniformly and spraying the mixture on the second semi-cured coating substrate, and semi-curing the mixture at room temperature to obtain a third semi-cured coating substrate;
[0040] (6) adding the surface raw material of the super-hydrophobic polyurethane layer to an organic solution of epoxy resin and its curing agent to obtain a fifth dissolved substance solution, wherein the surface raw material is a raw material that can form a super-hydrophobic structure on the surface of the polyurethane material;
[0041] (7) spraying the fifth dissolved substance solution onto the third semi-cured coating substrate and curing it at room temperature to obtain the composite self-healing anti-corrosion coating material;
[0042] The surface raw materials of the super-hydrophobic polyurethane layer include one or more of composite nanomaterials, precipitated calcium carbonate, carbon nanotubes, silicon nanomaterials, and one or more of fluorinated silane, tetraethyl orthosilicate and 1H,1H,2H,2H-perfluorodecyltriethoxysilane; the organic solution of the metal salt is an ethanol solution and / or a tetrahydrofuran solution of the metal salt; and the organic solution of the gas-phase nanomaterial and / or silicon nanomaterial is a tetrahydrofuran solution of the gas-phase nanomaterial and / or silicon nanomaterial.
[0043] Preferably, the paint layer includes a zinc-rich primer coating and a curing agent thereof.
[0044] Preferably, the step (6) specifically comprises:
[0045] Dispersing the super-hydrophobic material and fluorinated silane in a mixed solution of anhydrous ethanol and aqueous ammonia, then adding tetraethyl orthosilicate and 1H,1H,2H,2H-perfluorodecyltriethoxysilane, reacting at 25-35° C. to obtain a super-hydrophobic suspension;
[0046] dissolving the epoxy resin and its curing agent in an organic solvent to obtain an epoxy resin system solution;
[0047] Mixing the super-hydrophobic suspension with the epoxy resin system solution to obtain a super-hydrophobic mixed solution;
[0048] The obtained super-hydrophobic mixed liquid is added to the surface of the polyurethane material and cured to obtain the super-hydrophobic polyurethane layer.
[0049] The composite self-healing anti-corrosion coating material of the present invention has functional zoning and synergistic effects, and has high durability, high adhesion, super hydrophobicity, anti-corrosion and self-healing properties. The material introduces a variety of dynamic cross-linked networks of polar, flexible and rigid groups and branched structures, and can provide rapid self-repair capabilities through the synergistic effects between different groups and cross-linked networks.
[0050] In some preferred embodiments, the zinc-rich primer layer contained in the present invention can enhance the balance between rapid self-healing and high adhesion of the material.
[0051] The self-healing elastomer introduced into the composite self-healing anti-corrosion coating material of the present invention can self-heal under high salt and high humidity conditions, and the introduced super-hydrophobic polyurethane layer can effectively block the entry of corrosive substances, better protect the self-healing elastomer layer, and overall improve the corrosion resistance, self-healing properties and durability of the coating.
[0052] In some specific embodiments, the polyacrylate elastomer (B-PEA) obtained in the present invention can repair scratches in only 1.5 hours (room temperature), 1 hour (underwater), and 2 hours (saturated salt water), and has a high adhesion strength of more than 3.4 MPa, which can resist mechanical damage such as water splashing and scratches, and has good durability in high-salt and high-humidity environments.
[0053] In some specific embodiments, the introduction of the paint layer in the present invention significantly improves the adhesion between the coating and the substrate, so that the adhesion strength can reach 13 MPa.
[0054] In some embodiments, compared with the B-PEA coating without a superhydrophobic barrier layer, the introduction of the superhydrophobic polyurethane layer in the present invention greatly improves the low-frequency impedance modulus |Z| of the material. f-0.01Hz and salt solution resistance time, reaching 3.9×10 10 Ω·cm 2 and >3600 hours. At the same time, the introduction of the B-PEA self-healing elastomer layer enables the super-hydrophobic polyurethane layer to also have room temperature self-healing ability (1.5 hours), making it long-term |Z| f-0.01Hz and salt solution resistance time increased to 7.7×10 9 Ω·cm 2 and >3600 hours. The synergistic effect of the two enables the anti-corrosion coating system to exhibit a high level of long-term durability and self-healing ability.
[0055] The composite self-healing anti-corrosion coating material of the present invention can be used in various fields such as surface self-cleaning and anti-corrosion, and has a wide range of applications.
[0056] The preparation method of the invention is simple, can be directly realized by a spraying method, has simple procedures, is easy to operate, and has good product performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 It is a schematic diagram of the structure of a composite self-healing anti-corrosion coating material in a specific implementation manner.
[0058] Figure 2 Schematic diagram of the repair mechanism of the self-healing elastomer in a specific embodiment.
[0059] Figure 3 This is a diagram showing the self-repairing process of the self-repairing elastomer obtained in the example after scratching.
[0060] Figure 4 This is a comparison chart of the corrosion resistance of the anti-corrosion coating material in Example 8 with and without a self-healing elastomer layer in 3.5% NaCl solution.
[0061] Figure 5 This is a graph showing the change in contact angle of the material in Example 8 during the coating scratch-self-repair cycle.
[0062] Figure 6 This is a graph showing the rolling angle change of the material in Example 8 during the coating scratch-self-repair cycle.
[0063] Figure 7 is the |Z| of the material in Example 8 during the coating scratch-self-repair cycle f-0.01Hz Change graph. DETAILED DESCRIPTION
[0064] The present invention is described in detail below in conjunction with the embodiments and drawings, but it should be understood that the embodiments and drawings are only used to exemplify the present invention and do not constitute any limitation on the protection scope of the present invention. All reasonable changes and combinations within the scope of the inventive concept of the present invention fall within the protection scope of the present invention.
[0065] See attached Figure 1 In some specific embodiments, the composite self-healing anti-corrosion coating material of the present invention comprises in sequence: a base layer, a paint layer, a self-healing elastomer layer and a super-hydrophobic polyurethane layer.
[0066] Among them, the base layer can be formed by using, for example, a carbon steel sheet, and the paint layer thereon can be used as an anode protection layer to actively protect the carbon steel sheet from corrosion; the self-healing elastomer layer thereon can be used as a self-healing layer to provide self-healing ability for the coating material as a whole, and the super-hydrophobic polyurethane layer can be used as a barrier layer to effectively block water and corrosive substances outside the coating. The layers also have a synergistic effect, which can improve the corrosion resistance and long-term durability of the material as a whole.
[0067] The self-healing elastic elastomer layer is an acrylic elastomer (B-PEA), which can repair scratches in just 1.5 hours (room temperature), 1 hour (underwater), and 2 hours (saturated salt water), plus a high adhesion strength of 3.4MPa. This meets the requirements of practical applications. It can resist mechanical damage such as water splashing and scratches, and has good durability in high-salt and high-humidity environments.
[0068] The repair mechanism is as follows Figure 2 As shown, the composite self-healing anti-corrosion coating material of the present invention contains dynamic bonds such as coordination bonds, ionic bonds, and intermolecular van der Waals forces. After the coating is damaged, new bonds will be exchanged and linked between the broken dynamic bonds, thereby achieving the purpose of self-repair.
[0069] In some specific embodiments, the composite self-healing anti-corrosion coating material of the present invention can be prepared by the following preparation steps:
[0070] (1) mixing the epoxy zinc-rich primer and its curing agent in a mass ratio of 5:1 to obtain a first coating solution;
[0071] (2) using a spray gun to evenly spray the first coating solution on a 100 μm substrate, and leaving it at room temperature for 6 hours to obtain a first semi-cured coating substrate; the substrate material used is a carbon steel sheet;
[0072] (3) preparing a polyacrylate self-healing elastomer, namely the first product B-PEA;
[0073] (4) dissolving the first product B-PEA in THF to obtain a first solute solution, wherein the mass concentration of the first product in the first solute solution is 30-40 wt %;
[0074] (5) dissolving one or more of anhydrous cobalt chloride, anhydrous copper chloride, zinc chloride, ferric chloride, and lithium bis(difluorosulfonyl)imide in ethanol and / or tetrahydrofuran to obtain a second solute solution; the mass fraction of the solute in the second solute solution is 0.1%;
[0075] (6) dispersing gas-phase hydrophobic nano-silica in THF and ultrasonicating for 10 minutes to obtain a first dispersion solution; the dispersion concentration in the first dispersion solution is 5%-9%;
[0076] (7) adding the second dissolved substance solution to the first dispersed substance solution at a mass ratio of 1:250 to obtain a second coating solution; the mass concentration of the solute in the second coating solution is 25-30 wt %;
[0077] (8) using a spray gun to evenly spray the second coating solution on the first semi-cured coating substrate obtained in step (2), and leaving it at room temperature for 2 hours until the second coating solution is semi-cured to obtain a second semi-cured coating substrate with a thickness of 100 μm;
[0078] (9) dissolving 4.8 g of one or more of precipitated calcium carbonate, carbon nanotubes, silicon nanomaterials, and fluorinated silane in a mixed solution of anhydrous ethanol and aqueous ammonia, ultrasonically treating for 30 minutes to fully disperse them, then adding tetraethyl orthosilicate (TEOS) and 1.8 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane (PFTOS), and finally adding the remaining 3 mL of PFTOS, reacting at 30° C. for 2 hours to obtain a second product super hydrophobic suspension; the mass concentration of the solute in the second product super hydrophobic suspension is 7-15 wt %;
[0079] (10) dissolving an epoxy resin (E51 (618)) and a curing agent in THF at a mass ratio of 3:1 to obtain a third dissolved solution, wherein the mass concentration of the solute (epoxy resin and curing agent) in the third dissolved solution is 25-30 wt %;
[0080] (11) mixing the second product superhydrophobic suspension and the third solute solution in a mass ratio of 12:5 to obtain a fourth solute solution;
[0081] (12) mixing the anticorrosive polyurethane topcoat and its curing agent in a mass ratio of 15:1 to obtain a third coating solution, wherein the mass concentration of the solute in the third coating solution is 40%-45%;
[0082] (13) spraying a third coating solution onto the second semi-cured coating substrate obtained in step (8) with a spray gun, and leaving the solution at room temperature for 1 hour to semi-cured to obtain a third semi-cured coating substrate with a thickness of 50 μm;
[0083] (14) Spray the fourth dissolved substance solution onto the third semi-cured coating substrate using a spray gun, and cure at room temperature for 7 days to obtain the composite self-healing anti-corrosion coating material.
[0084] The total amount of initiators AIBN and BPO is 0.5% of the mass of the acrylate, and the total amount of chain transfer agents n-dodecyl mercaptan, KH580 and isopropanol is 1% of the mass of the acrylate.
[0085] Among them, the first product B-PEA has the following structural formula:
[0086]
[0087] in:
[0088] R1 is selected from any one of the following structures:
[0089]
[0090] R2 is selected from any one of the following structures:
[0091]
[0092] R3 is selected from any one of the following structures:
[0093]
[0094] R4 is selected from any one of the following structures:
[0095]
[0096] R5 is selected from any one of the following structures:
[0097]
[0098] and:
[0099] a:b:c:d=100:15-30:0.5-8:0.5-4.
[0100] Furthermore, the preparation of the polyacrylate self-healing elastomer is further described below in conjunction with the examples.
[0101] Example 1
[0102] The self-healing elastomer was prepared by the following steps:
[0103] Ethyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:20, and then 25 wt% acrylonitrile, 0.5 wt% 4-vinylpyridine, 0.5 wt% divinylbenzene, 0.5 wt% n-dodecyl mercaptan, 0.5 wt% 2,2'-azobisisobutyronitrile and 0.5 wt% BPO were added thereto according to the mass of ethyl acrylate. The solution was stirred at 70°C for 16 hours, and the solution was allowed to stand for 48 hours to obtain a transparent reaction solution. The reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, i.e., a self-healing elastomer B-PEA, and the structural formula of the elastomer is as follows:
[0104]
[0105] Among them, a:b:c:d=100:25:0.5:0.5.
[0106] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0107] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; anhydrous cobalt chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and the mixed solution was poured onto a mold after stirring at room temperature for 2 hours, and placed at 70°C for 12 hours to obtain a self-healing elastomer layer material B-PEA-0.5-Co.
[0108] Example 2
[0109] The self-healing elastomer was prepared by the following steps:
[0110] Butyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:20, and then 25 wt% acrylic acid, 1 wt% 4-vinylpyridine, 1 wt% divinylbenzene, 1 wt% n-dodecyl mercaptan, and 1 wt% 2,2'-azobisisobutyronitrile were added thereto, and the solution was stirred at 70°C for 24 hours. After that, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution, and the reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, namely, the self-healing elastomer B-PEA, the structural formula of which is as follows:
[0111]
[0112] Among them, a:b:c:d=100:25:1:1.
[0113] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0114] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; anhydrous cupric chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution and the first dispersion solution were added to the first dissolve solution at a mass ratio of 1:250, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 8 hours to obtain a self-healing elastomer layer material B-PEA-1-Cu.
[0115] Example 3
[0116] The self-healing elastomer was prepared by the following steps:
[0117] Isooctyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:20, and then 25 wt% acrylonitrile, 2 wt% 4-vinylpyridine, 2 wt% KH570, 2 wt% n-dodecyl mercaptan, 0.5 wt% 2,2'-azobisisobutyronitrile, and 0.5 wt% BPO were added thereto. After the solution was stirred at 70°C for 24 hours, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution. The reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, i.e., a self-healing elastomer B-PEA, the structural formula of which is as follows:
[0118]
[0119] Among them, a:b:c:d=100:25:2:2.
[0120] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0121] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; zinc chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 8 hours to obtain a self-healing elastomer layer material B-PEA-2-Zn.
[0122] Example 4
[0123] The self-healing elastomer was prepared by the following steps:
[0124] Butyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:15, and then 20 wt% benzyl methacrylate, 1 wt% 4-vinyl imidazole, 1 wt% KH570, 2 wt% n-dodecyl mercaptan, and 1 wt% 2,2'-azobisisobutyronitrile were added thereto. The solution was stirred at 70°C for 22 hours, and then the solution was allowed to stand for 48 hours to obtain a transparent reaction solution. The reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, i.e., a self-healing elastomer B-PEA, the structural formula of which is as follows:
[0125]
[0126] Among them, a:b:c:d=100:20:1:1.
[0127] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0128] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; zinc chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 9 hours to obtain a self-healing elastomer layer material B-PEA-1-Zn.
[0129] Example 5
[0130] The self-healing elastomer was prepared by the following steps:
[0131] Isooctyl acrylate and THF were added to a 50 mL round-bottom flask at a mass ratio of 1:15, and then 18 wt% of acrylic acid, 1 wt% of 4-vinylpyridine, 1 wt% of divinylbenzene, 1 wt% of n-dodecyl mercaptan, and 1 wt% of 2,2'-azobisisobutyronitrile were added thereto, and the solution was stirred at 70°C for 22 hours. After that, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution, and the reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, namely, the self-healing elastomer B-PEA, the structural formula of which is as follows:
[0132]
[0133] Among them, a:b:c:d=100:18:1:1.
[0134] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0135] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; anhydrous ferric chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 9 hours to obtain a self-healing elastomer layer material B-PEA-1-Fe.
[0136] Example 6
[0137] The self-healing elastomer was prepared by the following steps:
[0138] Ethyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:15, and then 20 wt% acrylonitrile, 5 wt% 4-vinylpyridine, 2 wt% divinylbenzene, 2 wt% KH580, and 1 wt% 2,2'-azobisisobutyronitrile were added thereto, and the solution was stirred at 70°C for 16 hours. After that, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution, and the reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, namely, the self-healing elastomer B-PEA, the structural formula of which is as follows:
[0139]
[0140] Among them, a:b:c:d=100:20:5:2.
[0141] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0142] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; anhydrous cobalt chloride was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 8 hours to obtain a self-healing elastomer layer material B-PEA-2-Co.
[0143] Example 7
[0144] The self-healing elastomer was prepared by the following steps:
[0145] Ethyl acrylate and 1,4-dioxane were added to a 50 mL round-bottom flask at a mass ratio of 1:20, and then 20 wt% of methyl acrylate, 8 wt% of 2-methyl-2-acrylic acid-2-(2-methoxyethoxy)ethyl ester, 1 wt% of divinylbenzene, 2 wt% of KH580, and 0.5 wt% of 2,2'-azobisisobutyronitrile were added thereto, and the solution was stirred at 70°C for 24 hours. After that, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution, and the reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, namely, the self-healing elastomer B-PEA, the structural formula of which is as follows:
[0146]
[0147] Among them, a:b:c:d=100:20:8:1.
[0148] Further, a self-healing elastomer layer is prepared according to the self-healing elastomer as follows:
[0149] The self-healing elastomer was dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica was dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of 9wt% of gas-phase nano-hydrophobic silica dispersion; lithium bis(difluorosulfonyl)imide was dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution was added to the first dissolve solution at a mass ratio of 1:250 to the first dispersion solution, and after stirring at room temperature for 2 hours, the obtained mixed solution was poured onto a mold and placed at 70°C for 8 hours to obtain a self-healing elastomer layer material B-PEA-1-Li with 8% 2-methyl-2-acrylic acid-2-(2-methoxyethoxy)ethyl ester.
[0150] Example 8
[0151] Based on the self-healing elastomer, a composite self-healing anti-corrosion coating material is prepared by the following steps:
[0152] 5 g of zinc-rich primer and 1 g of curing agent were mixed evenly, and then the obtained mixed solution was sprayed onto a carbon steel sheet with a spray gun at a pressure of 3-4 bar, and left at room temperature for 4 hours to obtain a substrate containing a semi-cured coating, i.e., a first semi-cured substrate;
[0153] Isooctyl acrylate and THF were added to a 50 mL round-bottom flask at a mass ratio of 1:20, and then 30 wt% acrylonitrile, 5 wt% 4-vinyl imidazole, 1 wt% divinylbenzene, 1 wt% KH580, and 0.5 wt% g 2,2'-azobisisobutyronitrile were added thereto, and the solution was stirred at 70°C for 22 hours. After that, the solution was allowed to stand for 48 hours to obtain a transparent reaction solution, and the reaction solution was precipitated 3 times with petroleum ether, and the obtained precipitate was dried under vacuum at 45°C to obtain a translucent solid, namely, the self-healing elastomer B-PEA, the structural formula of which is as follows:
[0154]
[0155] Among them, a:b:c:d=100:30:5:1.
[0156] The elastomer is dissolved in tetrahydrofuran to obtain a first dissolve solution with a concentration of 35wt%; gas-phase nano-hydrophobic silica is dispersed in THF, and ultrasonicated for 10 minutes to obtain a first dispersion concentration of gas-phase nano-hydrophobic silica dispersion with a concentration of 9wt%; anhydrous cobalt chloride is dissolved in THF to obtain a second dissolve solution with a concentration of 1wt%; the second dissolve solution and the first dispersion solution are added to the first dissolve solution at a mass ratio of 1:250, and the mixed solution is poured onto a mold after stirring at room temperature for 2 hours, and placed at 70°C for 9 hours to obtain a self-healing elastomer layer material B-PBA-1-Co;
[0157] Take 2g of the self-healing elastomer layer material B-PEA-1-Co, add 5g of tetrahydrofuran to completely dissolve it, then spray the obtained solution onto the first semi-cured substrate with a spray gun, and leave it at room temperature for 4 hours to semi-cure B-PEA-1-Co to obtain a second semi-cured substrate, i.e., EZ / B-PEA-1-Co substrate;
[0158] 7.5 g of waterborne polyurethane topcoat and 0.5 g of curing agent were mixed evenly, and then the obtained mixed solution was sprayed onto the EZ / B-PEA-1-Co substrate with a spray gun at a pressure of 3-4 bar, and left at room temperature for 2 hours to semi-cure the polyurethane topcoat, thereby obtaining a third semi-cured substrate, i.e., the EZ / B-PEA-1-Co / PU substrate;
[0159] 4.8 g of silicon nanomaterial and fluorinated silane were dissolved in a mixed solution of anhydrous ethanol and ammonia water, and ultrasonicated for 30 minutes to fully disperse them, and then tetraethyl orthosilicate (TEOS) and a portion of 1H,1H,2H,2H-perfluorodecyltriethoxysilane (PFTOS) (1.8 mL) were added, and finally, the remaining PFTOS (3 mL) was added, and reacted at 30° C. for 2 hours to obtain a second product super hydrophobic suspension with a concentration of 7-15 wt %;
[0160] Take 3g of epoxy resin and 1g of its curing agent, dissolve them in a mass ratio of 1:5 between the total mass of the epoxy resin and the curing agent and THF, then add 23g of superhydrophobic suspension and mix evenly, use a spray gun to spray the obtained mixed system on the EZ / B-PEA-1-Co / PU substrate at a pressure of 3-4 bar, and leave it at room temperature for 7 days to completely cure the system to obtain a composite self-healing anti-corrosion coating material EZ / B-PEA-1-Co / SN.
[0161] The elastomer obtained in the above examples 1-7 (i.e., B-PEA) was subjected to a self-healing test. The test method was as follows: the elastomer was cut with a utility knife to form cracks with a spacing of 1-2 mm, and then placed at room temperature and underwater, respectively. The cracks were observed for 24 hours using a BX51-P optical microscope to observe the self-healing behavior of the elastomer. Among them, the coating only takes 1.5 hours (room temperature), 1 hour (underwater), and 2 hours (salt water) to repair scratches. For example, as shown in the attached figure, Figure 3 As shown, it can be seen that it has excellent self-healing ability.
[0162] The anti-corrosion performance of the EZ / B-PEA-1-Co material obtained in Example 8 above was tested in the following manner: the composite self-healing anti-corrosion coating material with the second semi-cured substrate EZ / B-PEA-1-Co and the anti-corrosion coating material prepared in the same manner but without the substrate were immersed in a 3.5wt% NaCl aqueous solution to test their anti-corrosion performance. The results are shown in the attached figure. Figure 4 As shown, it can be seen that after immersion in NaCl aqueous solution, the coating material with the addition of EZ / B-PEA-1-Co substrate was not corroded, while the coating material without the substrate was corroded, indicating that the addition of EZ / B-PEA-1-Co improved the corrosion resistance and long-term durability of the coating.
[0163] The hydrophobic performance of the EZ / B-PEA-1-Co / SN coating material obtained in Example 8 above was tested by using Sindin SDC-350 to test the contact angle (CA) and rolling angle (SA) of the material. All contact angle tests were performed using 5 μL of water drops, and each measured value was equal to the average value of the measurements at 5 points on the surface. The results are shown in the attached figure. Figure 5 And attached Figure 6 As shown, it can be seen that after 5 damage-repair cycles, the hydrophobic performance of the EZ / B-PEA-1-Co / SN coating material is still CA>150° and SA<10°, indicating that it has excellent durability.
[0164] The electrochemical performance of the EZ / B-PEA-1-Co / SN coating material obtained in Example 8 was tested by using a CHI660E electrochemical workstation to measure the polarization curve of the sample with a 3.5wt% NaCl aqueous solution as the electrolyte solution through a three-electrode system. In the three-electrode system, the sample was used as the working electrode, the saturated calomel electrode (SCE) was used as the reference electrode, and the platinum electrode was used as the counter electrode. The frequency range of EIS was 10 5 ~10 -2 Hz, with a sinusoidal disturbance of 10 mV amplitude. All EIS data were fitted using Zview software, and the results are shown in the attached Figure 7 As shown in Table 1, it can be seen that after 5 damage-repair cycles, the impedance of the EZ / B-PEA-1-Co / SN coating material is still >10 10 , indicating that it has excellent durability and excellent barrier properties.
[0165] Table 1 shows the |Z| of the coating in 3.5% sodium chloride solution with immersion time f-0.01Hz change.
[0166]
[0167] As shown in Table 1, after 150 days of exposure to 3.5% sodium chloride solution, the impedance of the EZ / B-PEA-1-Co / SN coating material is still >10 10 , it can be seen that the EZ / B-PEA-1-Co / SN coating material has excellent barrier properties. Even in the presence of scratches, after 150 days of immersion, the impedance of the EZ / B-PEA-1-Co / SN coating material is still >10 9 ,It can be seen that the EZ / B-PEA-1-Co / SN coating material is resistant to mechanical damage such as scratches, and has good durability in high salt and high humidity environments, which greatly prolongs the service life of the coating.
[0168] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A composite self-healing anti-corrosion coating material, characterized in that: It comprises in sequence: a base layer, a paint layer, a self-healing elastomer layer and a super-hydrophobic polyurethane layer, wherein the self-healing elastomer layer comprises a polyacrylate elastomer and a metal salt and a gas-phase nanomaterial and / or a silicon nanomaterial having the following structure: in: R1 is selected from any one of the following structures: R2 is selected from any one of the following structures: R3 is selected from any one of the following structures: R4 is selected from any one of the following structures: R5 is selected from any one of the following structures: And, a:b:c:d=100:(15-30):(0.5-8):(0.5-4); The super-hydrophobic polyurethane layer comprises a polyurethane material having a super-hydrophobic material distributed on the surface, wherein the super-hydrophobic material is selected from one or more of precipitated calcium carbonate, carbon nanotubes, and silicon nanomaterials; the self-healing elastomer layer is prepared by a preparation method comprising the following processes: the metal salt is selected from one or more of cobalt chloride, copper chloride, zinc chloride, ferric chloride, and lithium bis(difluorosulfonyl)imide; The raw material components A, B, C, D and E of the polyacrylate elastomer are mixed, reacted at 65-75° C. and then allowed to stand to obtain a transparent reaction solution, the obtained reaction solution is precipitated with petroleum ether, the obtained precipitate is vacuum dried and dissolved in an organic solvent, and then a dispersion of gas-phase nanomaterials and / or silicon nanomaterials and an organic solution of metal salts are added, mixed evenly and added to a mold, and cured at 65-75° C. to obtain the self-healing elastomer layer; Wherein, the component A is selected from one or more of methyl acrylate, ethyl acrylate, butyl acrylate, and isooctyl acrylate; the component B is selected from one or more of acrylonitrile, acrylic acid, benzyl methacrylate, and 2-methyl-2-acrylic acid-2-(2-methoxyethoxy)ethyl ester; the component C is selected from 1,4-dioxane and / or tetrahydrofuran; the component D is selected from one or more of 4-vinylpyridine, 4-vinylimidazole, divinylbenzene, and n-dodecyl mercaptan; the component E is selected from 2,2'-azobisisobutyronitrile and / or dibenzoyl peroxide; and the mass ratio of the component A to the component B is 1:0.1 to 0.
5.
2. The composite self-healing anti-corrosion coating material according to claim 1, characterized in that: The raw material of the polyacrylate elastomer further includes component F, and the component F is selected from silane coupling agents.
3. The composite self-healing anti-corrosion coating material according to claim 1, characterized in that: The gas phase nano material is selected from gas phase hydrophobic silica and / or gas phase white carbon black.
4. The composite self-healing anti-corrosion coating material according to claim 1, characterized in that: The super hydrophobic material is distributed in the epoxy resin system, and the epoxy resin system is fixed on the surface of the polyurethane material.
5. The composite self-healing anti-corrosion coating material according to claim 1, characterized in that: in, The base layer is formed of a carbon steel sheet; and / or the paint layer comprises a zinc-rich primer.
6. The method for preparing the composite self-healing anti-corrosion coating material according to claim 1, characterized in that: It includes the following steps: (1) forming a semi-cured paint layer on the base layer by spraying to obtain a first semi-cured coating base; (2) mixing the raw material components of the polyacrylate elastomer, reacting them at 65-75° C., and then standing to obtain a transparent reaction solution, precipitating the obtained reaction solution with petroleum ether, vacuum drying the obtained precipitate, and then dissolving it in an organic solvent to obtain a first dissolved solution; (3) adding metal salt and / or organic solution of metal salt and organic solution of gas phase nanomaterial and / or silicon nanomaterial to the first dissolved substance solution to obtain a second coating solution; (4) spraying the second coating solution onto the first semi-cured coating substrate and semi-curing at room temperature to obtain a second semi-cured coating substrate; (5) mixing the polyurethane coating and the curing agent uniformly and spraying the mixture on the second semi-cured coating substrate, and semi-curing the mixture at room temperature to obtain a third semi-cured coating substrate; (6) adding the surface raw material of the super hydrophobic polyurethane layer to an organic solution of epoxy resin and its curing agent to obtain a fifth dissolved substance solution; (7) spraying the fifth dissolved substance solution onto the third semi-cured coating substrate and curing it at room temperature to obtain the composite self-healing anti-corrosion coating material; The surface raw materials of the super-hydrophobic polyurethane layer include one or more of composite nanomaterials, precipitated calcium carbonate, carbon nanotubes, silicon nanomaterials, and one or more of fluorinated silane, tetraethyl orthosilicate and 1H,1H,2H,2H-perfluorodecyltriethoxysilane; the organic solution of the metal salt is an ethanol solution and / or a tetrahydrofuran solution of the metal salt; and the organic solution of the gas-phase nanomaterial and / or silicon nanomaterial is a tetrahydrofuran solution of the gas-phase nanomaterial and / or silicon nanomaterial.
7. The preparation method according to claim 6, characterized in that: The paint layer comprises a zinc-rich primer coating and a curing agent thereof.
8. The preparation method according to claim 6, characterized in that: The step (6) specifically comprises: Dispersing the super-hydrophobic material and fluorinated silane in a mixed solution of anhydrous ethanol and aqueous ammonia, then adding tetraethyl orthosilicate and 1H,1H,2H,2H-perfluorodecyltriethoxysilane, reacting at 25-35° C. to obtain a super-hydrophobic suspension; dissolving the epoxy resin and its curing agent in an organic solvent to obtain an epoxy resin system solution; Mixing the super-hydrophobic suspension with the epoxy resin system solution to obtain a super-hydrophobic mixed solution; The obtained super-hydrophobic mixed liquid is added to the surface of the polyurethane material and cured to obtain the super-hydrophobic polyurethane layer.
Citation Information
Patent Citations
Super-hydrophobic composite anti-corrosion coating as well as construction method and application thereof
CN114686103A
Polyurethane-based self-repairing super-hydrophobic coating and preparation method thereof
CN116120827A
Preparation method of pipeline steel-based underwater synergistic self-repairing super-hydrophobic coating
CN116285628A
Self-healing material, coating composition including self-healing material, and steel plate including coating composition membrane
KR101372758B1
Functional self-healing coatings and compositions and methods for forming such coatings
US20170051157A1