Preparation method and application of zinc metal anode modified with composite organic coating

By coating the zinc metal anode surface with a composite coating of polymer and conductive polyaniline, the problems of zinc dendrites and corrosion were solved, the coulombic efficiency and cycle performance of zinc-ion batteries were improved, and a stable zinc deposition/stripping process was achieved.

CN116799192BActive Publication Date: 2026-11-10HEBEI UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311007397.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2026-11-10
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

In aqueous zinc-ion batteries, zinc metal anodes suffer from zinc dendrite growth and electrode/electrolyte interface side reactions, leading to reduced coulombic efficiency and poor cycle performance. Furthermore, existing polymer coatings have poor ionic conductivity, making it difficult to achieve a stable zinc deposition/stripping process at high current densities.

Method used

A composite organic coating is used to modify the zinc metal anode. By coating the zinc foil surface with a mixed solution of polymer and conductive polyaniline, a uniform and dense coating is formed. Combining the mechanical properties of the polymer and the high conductivity of the conductive polyaniline, zinc dendrites and corrosion are suppressed, and zinc ion distribution and transport are optimized.

Benefits of technology

It effectively inhibits zinc dendrites and corrosion, improves the coulombic efficiency of zinc metal anode, enables stable cycling of the battery at high coulombic efficiency, extends battery life, and has a simple and easy preparation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116799192B_ABST
    Figure CN116799192B_ABST
Patent Text Reader

Abstract

A method for preparing and applying a zinc metal anode modified with a composite organic coating is disclosed. The method includes the following steps: adding a polymer and polyaniline to an organic solvent to obtain a mixed solution; then coating the mixed solution onto the surface of a pretreated zinc foil, followed by vacuum drying to obtain the zinc metal anode modified with a composite organic coating. The polyaniline is conductive polyaniline; the polymer is one or more of polyvinyl butyral, polyvinyl chloride, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate. This invention provides a simple preparation method using inexpensive and readily available raw materials, and has significant value for the practical application of zinc metal anodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of zinc metal anode preparation technology for aqueous zinc-ion batteries, specifically relating to a zinc metal anode modified with a composite organic coating, its preparation method, and its application. Background Technology

[0002] Aqueous zinc-ion batteries have attracted much attention due to their advantages such as low cost, high safety, high power density, and environmental friendliness. However, zinc metal anodes face problems such as zinc dendrite growth and electrode / electrolyte interface side reactions in neutral and weakly acidic electrolytes, leading to reduced battery coulombic efficiency, poor cycle performance, and the gases generated by the side reactions may further pose safety hazards.

[0003] Currently, various methods and strategies have been proposed to improve the safety and cycle life of zinc metal anodes, such as surface modification, structural design, electrolyte optimization, and separator optimization. Among these, surface coating modification is the most common, simplest, and most effective method, utilizing a protective coating to prevent direct contact between the zinc anode and the electrolyte. The coating not only separates the electrolyte from the zinc anode but also acts as an ion sieve, regulating the electrochemical environment on the anode surface, inducing uniform zinc ion deposition, reducing dendrite formation, and improving battery life. In recent years, various surface protective layers have been developed and utilized, and their improvement effect on zinc metal anodes is closely related to the characteristics of the protective layer, such as organic layers, inorganic layers, and organic / inorganic composite layers. Polyacrylonitrile, polyvinyl butyral, and polyvinyl chloride polymers exhibit good corrosion resistance in aqueous electrolytes. WEI et al. (patent number CN112490396-A) prepared a zinc metal anode modified with a polyacrylonitrile coating by pre-oxidizing polyacrylonitrile in an air atmosphere at a temperature of 150-500℃. The organic coating based on the modified polyacrylonitrile can protect the zinc anode from electrolyte corrosion. However, the poor ionic conductivity of polymers easily leads to an increase in polarization voltage, making it difficult to achieve a stable zinc deposition / stripping process under high current density conditions.

[0004] To address the above problems, this invention provides a method for preparing a zinc metal anode modified with a composite organic coating. The excellent mechanical properties and corrosion resistance of the polymer can effectively inhibit the formation of zinc dendrites. Simultaneously, conductive polyaniline possesses good conductivity and ion adsorption properties, which can improve the distribution and transport of zinc ions at the electrode / electrolyte interface, effectively improving the electrochemical performance of zinc-ion batteries. This method is simple, easy to control, and can prepare zinc metal anodes with excellent electrochemical performance and high stability. Summary of the Invention

[0005] The purpose of this invention is to address the technical problems in the preparation of zinc metal anodes in aqueous zinc-ion batteries by providing a method for preparing and applying a zinc metal anode modified with a composite organic coating. This method modifies the polymer by adding conductive polyaniline, combining the excellent mechanical properties of the polymer with the high conductivity of conductive polyaniline, effectively solving problems such as dendrite formation and corrosion in zinc metal anodes. The preparation method of this invention is simple, and the raw materials are inexpensive and readily available, making it of significant value for the practical application of zinc metal anodes.

[0006] The technical solution of this invention is as follows:

[0007] A method for preparing a zinc metal anode modified with a composite organic coating, the method comprising the following steps:

[0008] (1) Zinc foil surface pretreatment to remove surface impurities;

[0009] (2) Add the polymer and substance A to an organic solvent and stir at 40-90°C for 0.5-20 h to obtain a mixed solution;

[0010] The mass ratio of the polymer to the organic solvent is 1:5 to 1:20; the mass ratio of the polymer to substance A is 50:1 to 5:1.

[0011] The substance A is polyaniline or doped polyaniline; the polymer is one or more of polyvinyl butyral, polyvinyl chloride, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate.

[0012] (3) The mixed solution obtained in step (2) is coated on the surface of the pretreated zinc foil and dried under vacuum to obtain a zinc metal anode modified with a composite organic coating; the coating thickness is 50-300 μm.

[0013] The doped polyaniline mentioned in step (2) is one or more of the following: sulfonic acid doped polyaniline, dodecylbenzenesulfonic acid doped polyaniline, hydrochloric acid doped polyaniline, phytic acid doped polyaniline, and phosphate doped polyaniline.

[0014] The organic solvent mentioned in step (2) is one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, and acetone.

[0015] The average molecular weight of the polymer mentioned in step (2) is 10,000 to 500,000;

[0016] In step (3), the vacuum drying temperature is 60-90℃ and the vacuum drying time is 6-18h.

[0017] The zinc metal anode modified with a composite organic coating prepared by the method is used as an anode in aqueous zinc-ion batteries.

[0018] The aforementioned aqueous zinc-ion battery uses CNT / MnO2 as the active positive electrode material to prepare the positive electrode, and employs a 2 mol / L electrolyte. -1 ZnSO4 and 0.1 mol L -1 A mixed aqueous solution of MnSO4 was assembled into a CR2016 coin cell using glass fiber as a separator.

[0019] The beneficial effects of this invention are as follows:

[0020] 1. This invention provides a novel method for modifying zinc metal anodes with composite organic coatings, namely, preparing composite organic coatings using polymers and conductive polyaniline.

[0021] 2. This invention utilizes a high molecular polymer as the substrate for the coating, which has good mechanical properties and corrosion resistance, and can effectively suppress the dendrite formation of zinc metal negative electrode and electrolyte corrosion problems.

[0022] 3. This invention uses conductive polyaniline as a high conductivity material, which can effectively improve the zinc ion transport kinetics of the coating and optimize the zinc ion deposition behavior, thereby effectively improving the coulombic efficiency of the zinc metal anode. The battery can maintain a high coulombic efficiency of 97% and cycle stably for more than 150 times.

[0023] 4. The preparation method of this invention is simple, mainly reflected in the fact that a mixed solution is obtained by simple heating and stirring, and then a composite organic coating can be prepared on the zinc anode by vacuum drying using a coating method. Attached Figure Description

[0024] Figure 1 SEM image of the zinc metal anode modified with the composite organic coating of Example 1;

[0025] Figure 2 Infrared spectrum image of the zinc metal anode modified with the composite organic coating of Example 1;

[0026] Figure 3 The corrosion resistance of the zinc metal anode modified with the composite organic coating in Example 1;

[0027] Figure 4 Symmetrical battery cycle stability of the zinc metal anode modified with a composite organic coating in Example 1;

[0028] Figure 5 SEM image of the zinc metal anode modified with the composite organic coating in Example 2;

[0029] Figure 6Infrared spectrum image of the zinc metal anode modified with the composite organic coating in Example 2;

[0030] Figure 7 To demonstrate the corrosion resistance of the zinc metal anode modified with the composite organic coating in Example 2;

[0031] Figure 8 The symmetrical battery cycle stability of the zinc metal anode modified with the composite organic coating in Example 2;

[0032] Figure 9 The coulombic efficiency curve of the zinc metal anode modified with the composite organic coating in Example 2 is shown. Detailed Implementation

[0033] The following examples are intended to further illustrate the present invention, but not to limit it.

[0034] Example 1:

[0035] The first step is to pre-treat the zinc foil surface to remove impurities. The specific steps are as follows:

[0036] Zinc sheets were soaked in 1 wt.% hydrochloric acid solution for 10 min, rinsed three times with deionized water, then rinsed three times with anhydrous ethanol, and dried at 60℃ for 2 h to obtain pretreated zinc sheets.

[0037] The second step involves dissolving the polymer and polyaniline in an organic solvent to prepare a mixed solution. The specific steps are as follows:

[0038] 0.3 g of polyacrylonitrile (average molecular weight 150,000) and 0.033 g of polyaniline were added to 3 g of N-methylpyrrolidone and stirred at 40 °C for 10 h to obtain a mixed solution.

[0039] The third step is to coat the mixed solution obtained in the second step onto the surface of zinc metal to prepare an organically coated zinc metal anode. The specific steps are as follows:

[0040] The mixed solution was uniformly coated onto the pretreated zinc metal surface using a scraper (coating thickness 100 μm), and then vacuum dried at 60 °C for 10 h to obtain a zinc metal anode modified with a composite organic coating.

[0041] The morphology of the sample was observed using a JEOL 7610F scanning electron microscope (SEM) from Japan. A uniform and dense coating was found on the zinc metal surface. Figure 1 The composite organic coating was tested using a VERTEX 80 / 80V Fourier transform infrared spectroscopy system, and the results are as follows: Figure 2 As shown, the wavenumber is 2246 cm⁻¹. -1 The absorption peak is a characteristic peak of the -C≡N- group, belonging to PAN polymers, at 1125 cm⁻¹.-1 The peak observed is characteristic of PANI and is attributed to -NH ●+ The vibration indicated successful preparation of the PAN / PANI composite. The Tafel curve of the zinc metal anode modified with the composite organic coating was tested using a CHI760E electrochemical workstation, which mainly reflects the corrosion resistance of the coating. The working electrode was zinc, the counter electrode was Pt, and the reference electrode was a saturated calomel electrode. The corrosion current density of the zinc metal anode was calculated to be 4.723 mA cm⁻¹ based on the Tafel curve test. -2 ( Figure 3 Studies suggest that a higher corrosion potential indicates a weaker tendency for corrosion, while a lower corrosion current corresponds to a lower corrosion rate. The prepared zinc metal anode, when used in a symmetrical battery, exhibited better cycle stability compared to a pure zinc symmetrical battery. Constant current charge-discharge tests were performed using the Xinwei Battery testing system; for the symmetrical battery, a 1mA cm⁻¹ current was achieved. -2 At current density, 1mAh cm -2 At the given surface capacity, stable cycling for 500 hours ( Figure 4 ).

[0042] Example 2:

[0043] The first step is to pre-treat the zinc foil surface to remove impurities. The specific steps are as follows:

[0044] Zinc sheets were soaked in 1 wt.% hydrochloric acid solution for 10 min, rinsed three times with deionized water, then rinsed three times with anhydrous ethanol, and dried at 60℃ for 2 h to obtain pretreated zinc sheets.

[0045] The second step involves dissolving the polymer and polyaniline in an organic solvent to prepare a mixed solution. The specific steps are as follows:

[0046] 0.3 g of polyacrylonitrile (average molecular weight 150,000) and 0.017 g of polyaniline were added to 3 g of N-methylpyrrolidone and stirred at 40 °C for 10 h to obtain a mixed solution.

[0047] The third step is to coat the mixed solution obtained in the second step onto the surface of zinc metal to prepare an organically coated zinc metal anode. The specific steps are as follows:

[0048] The mixed solution was uniformly coated onto the pretreated zinc metal surface using a scraper (coating thickness 100 μm), and then vacuum dried at 60 °C for 10 h to obtain a zinc metal anode modified with a composite organic coating.

[0049] The morphology of the sample was observed using a JEOL 7610F scanning electron microscope (SEM) from Japan. A uniform and dense coating was found on the zinc metal surface. Figure 5The composite organic coating was tested using a VERTEX 80 / 80V Fourier transform infrared spectroscopy system, and the results are as follows: Figure 6 As shown, the spectrum simultaneously exhibits characteristic peaks of both polymers, with a wavenumber of 2240 cm⁻¹. -1 The absorption peak is a characteristic peak of the -C≡N- group, belonging to PAN polymers, at 1138 cm⁻¹. -1 The peak observed is characteristic of PANI and is attributed to -NH ●+ The vibration indicated successful preparation of the PAN / PANI composite. The Tafel curve of the zinc metal anode modified with the composite organic coating was tested using a CHI760E electrochemical workstation, which mainly reflects the corrosion resistance of the coating. The working electrode was zinc, the counter electrode was a Pt electrode, and the reference electrode was a saturated calomel electrode. The corrosion current density of the zinc metal anode was calculated to be 4.148 mA cm⁻¹ from the Tafel curve test. -2 ( Figure 7 The prepared zinc metal anode was used in a symmetrical battery, exhibiting better cycle stability compared to a pure zinc symmetrical battery. Constant current charge-discharge tests were performed using the Xinwei Battery Testing System; for the symmetrical battery, a constant current charge-discharge test could be conducted at 1 mA cm⁻¹. -2 At current density, 1mAh cm -2 Stable cycling for 800 hours at the given surface capacity. Figure 8 The coulombic efficiency of the zinc anode was tested by assembling a half-cell with Zn and Cu electrodes. During the discharge process of the half-cell, Zn... 2+ The zinc electrode detaches and deposits Zn on the Cu electrode surface, bypassing the separator. During charging, it is redeposited on the Zn electrode surface. Coulomb efficiency is calculated as the ratio of Zn stripped from and deposited on the Cu electrode during one charge-discharge cycle. By comparing the change in coulomb efficiency, we can understand the Zn deposition process during charge-discharge. 2+ The reversibility and stability of the electrode stripping deposition reaction are used to determine the effect of the organic coating on Zn. 2+ The regulatory effect on the movement process. The results are as follows: Figure 9 As shown, at a current density of 1 mA cm⁻¹ -2 The capacity density is 1 mAh cm⁻¹ -2 Under these conditions, the battery can maintain a high coulombic efficiency of 97% and cycle stably for more than 140 times.

[0050] Example 3:

[0051] The first step is to pre-treat the zinc foil surface to remove impurities. The specific steps are as follows:

[0052] Zinc sheets were soaked in 1 wt.% hydrochloric acid solution for 10 min, rinsed three times with deionized water, then rinsed three times with anhydrous ethanol, and dried at 60℃ for 2 h to obtain pretreated zinc sheets.

[0053] The second step involves dissolving the polymer and doped polyaniline in an organic solvent to prepare a mixed solution. The specific steps are as follows:

[0054] 0.3 g of polymethyl methacrylate (average molecular weight 120,000) and 0.022 g of dodecylbenzenesulfonic acid-doped polyaniline were added to 4 g of N,N-dimethylformamide and stirred at 40 °C for 5 h to obtain a mixed solution.

[0055] The third step is to coat the mixed solution obtained in the second step onto the surface of zinc metal to prepare an organically coated zinc metal anode. The specific steps are as follows:

[0056] The mixed solution was uniformly coated onto the pretreated zinc metal surface using a scraper (coating thickness 150 μm), and then vacuum dried at 60 °C for 10 h to obtain a zinc metal anode modified with a composite organic coating.

[0057] Example 4:

[0058] The first step is to pre-treat the zinc foil surface to remove impurities. The specific steps are as follows:

[0059] Zinc sheets were soaked in 1 wt.% hydrochloric acid solution for 10 min, rinsed three times with deionized water, then rinsed three times with anhydrous ethanol, and dried at 60℃ for 2 h to obtain pretreated zinc sheets.

[0060] The second step involves dissolving the polymer and doped polyaniline in an organic solvent to prepare a mixed solution. The specific steps are as follows:

[0061] 0.3 g of polyvinylidene fluoride (average molecular weight 180,000) and 0.017 g of phytic acid-doped polyaniline were added to 3 g of N-methylpyrrolidone and stirred at 60 °C for 1 h to obtain a mixed solution.

[0062] The third step is to coat the mixed solution obtained in the second step onto the surface of zinc metal to prepare an organically coated zinc metal anode. The specific steps are as follows:

[0063] The mixed solution was uniformly coated onto the pretreated zinc metal surface using a scraper (coating thickness 200 μm), and then vacuum dried at 80 °C for 12 h to obtain a zinc metal anode modified with a composite organic coating.

[0064] The purpose of this invention is to address the technical challenges in preparing zinc metal anodes for aqueous zinc-ion batteries by providing a composite organic coating-modified zinc metal anode. This method combines the excellent mechanical properties of polymers with the high conductivity of conductive polyaniline, effectively solving problems such as dendrite formation and corrosion in zinc metal anodes. Furthermore, the preparation method is simple, and the raw materials are inexpensive and readily available, making it of significant value for the practical application of zinc metal anodes.

[0065] Matters not covered in this invention are common knowledge.

Claims

1. A method for preparing a zinc metal anode modified with a composite organic coating, characterized in that the method includes the following steps: (1) Zinc foil surface pretreatment to remove surface impurities; (2) Add the polymer and substance A to an organic solvent and stir at 40~90℃ for 0.5~20 h to obtain a mixed solution; The mass ratio of the polymer to the organic solvent is 1:5 to 1:20; the mass ratio of the polymer to substance A is 50:1 to 5:

1. The substance A is polyaniline or doped polyaniline; the polymer is one or more of polyvinyl butyral, polyvinyl chloride, polyacrylonitrile, and polymethyl methacrylate. (3) The mixed solution obtained in step (2) is coated on the surface of the pretreated zinc foil and dried under vacuum to obtain a zinc metal anode modified with a composite organic coating; the coating thickness is 50~300μm. The doped polyaniline mentioned in step (2) is one or more of the following: sulfonic acid doped polyaniline, dodecylbenzenesulfonic acid doped polyaniline, hydrochloric acid doped polyaniline, phytic acid doped polyaniline, and phosphoric acid doped polyaniline; The organic solvent mentioned in step (2) is one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, and acetone.

2. The method for preparing the zinc metal anode modified with a composite organic coating as described in claim 1, characterized in that: The average molecular weight of the polymer mentioned in step (2) is 10,000 to 500,000.

3. The method for preparing the zinc metal anode modified with a composite organic coating as described in claim 1, characterized in that: In step (3), the vacuum drying temperature is 60~90℃ and the vacuum drying time is 6~18h.

4. The application of the composite organic coating modified zinc metal anode prepared by the method of claim 1, characterized in that it is used as an anode in an aqueous zinc-ion battery.

5. The application as described in claim 4, characterized in that the aqueous zinc-ion battery uses CNT / MnO2 as the active positive electrode material to prepare the positive electrode, and the electrolyte uses 2 mol / L... -1 ZnSO4 and 0.1 mol L -1 A mixed aqueous solution of MnSO4 was assembled into a CR2016 coin cell using glass fiber as a separator.

Citation Information

Patent Citations

  • Zinc electrode, and preparation method and application thereof

    CN112886079A

  • Application of ordered conjugated polymer material in protecting zinc negative electrode

    CN116154118A