A self-repairing admixture for cracks in composite concrete materials and its application

Through plant urease-induced calcium carbonate precipitation and magnesium oxide modification technology, self-healing of concrete is achieved, solving the problem of difficulty in repairing internal cracks in concrete in the existing technology, improving impermeability and durability, and reducing repair costs.

CN116803943BActive Publication Date: 2024-10-22SHANDONG EXPRESSWAY INFRASTRUCTURE CONSTR CO LTD +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310814958.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-10-22
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

It is difficult to effectively repair internal cracks in concrete with existing technology, and commonly used repair methods are costly and inefficient, and cannot effectively improve the impermeability and durability of concrete.

Method used

Plant urease is used as the source of urease, combined with the calcium source of the concrete itself, and urease is induced to produce calcium carbonate crystals for crack repair. Magnesium oxide is added to modify the concrete, and the urease-induced calcium carbonate precipitation technology is used in conjunction with the urease-induced calcium carbonate precipitation technology to achieve self-healing of concrete.

Benefits of technology

Significantly improve the self-healing ability of concrete, reduce crack generation, enhance impermeability and waterproof performance, reduce repair costs, meet project needs, and improve project quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116803943B_ABST
    Figure CN116803943B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-cost-effective composite concrete material crack self-repairing admixture and its application, and belongs to the technical field of waterproof concrete materials. The high-cost-effective composite concrete material crack self-repairing admixture includes plant urease. The present invention selects watermelon seeds with rich plant urease content and low cost as the source of urease, and uses concrete itself as the calcium source. After the concrete cracks are generated, urease induces the production of calcium carbonate crystals with gelling properties to complete the crack repair. At the same time, an appropriate amount of magnesium oxide is added to modify the concrete, and the urease-induced calcium carbonate precipitation technology is used to complete the self-healing of microcracks inside and on the surface of the concrete, and the present invention is the first to use urease to induce calcium carbonate precipitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waterproof concrete materials, and in particular to a high-cost-performance composite concrete material crack self-repairing admixture and application thereof. Background Art

[0002] Concrete is a bonding material used in construction. It is made of a certain proportion of fine aggregate and cement. It is widely used in the construction industry for its low cost and high strength. During its molding process, cracks often occur due to factors such as uneven settlement and differences in temperature and humidity between the surface and the interior. These microcracks will become channels for moisture and harmful substances to enter the concrete, reducing the concrete's impermeability and strength, and seriously damaging the durability of concrete masonry. If these cracks are allowed to develop, it will inevitably cause serious economic losses.

[0003] Concrete cracks are inevitable. How to repair concrete cracks and reduce the number of cracks as much as possible is of great significance. At present, the commonly used repair technologies at home and abroad mainly focus on surface spraying. The implementation of this technology not only consumes a lot of manpower, material and financial resources to regularly maintain concrete, but also cannot effectively repair the internal cracks of cement concrete. Summary of the invention

[0004] The purpose of the present invention is to provide a cost-effective composite concrete material crack self-repairing admixture and its application to solve the problems existing in the above-mentioned prior art. The present invention selects watermelon seeds with rich plant urease content and low cost as the source of urease, and uses concrete itself as the calcium source. After the concrete cracks are generated, urease induces the production of calcium carbonate crystals with gelling properties to complete the crack repair. At the same time, an appropriate amount of magnesium oxide is added to modify the concrete, and the urease-induced calcium carbonate precipitation technology is used to complete the self-healing of microcracks inside and on the surface of the concrete. In addition, the present invention is the first to use urease to induce calcium carbonate precipitation.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is a cost-effective composite concrete material crack self-repairing admixture, wherein the admixture comprises plant urease.

[0007] Furthermore, the plant urease is provided by watermelon seeds.

[0008] Furthermore, the cost-effective composite concrete material crack self-repairing admixture also includes magnesium oxide as a component of the admixture.

[0009] The second technical solution of the present invention: an application of the above-mentioned cost-effective composite concrete material crack self-repairing admixture in a self-repairing concrete material.

[0010] Furthermore, the raw materials for preparing the self-repairing concrete material include any one of the following:

[0011] The first type includes the following raw materials by weight: 320 parts of cement, 60 parts of fly ash, 40 parts of mineral powder, 728 parts of sand, 1092 parts of gravel, 160 parts of water, 4.2 parts of water reducer, 4.2 parts of urea and 0.0063 parts of plant urease;

[0012] The second type includes the following raw materials in parts by mass: 320 parts of cement, 60 parts of fly ash, 40 parts of mineral powder, 728 parts of sand, 1092 parts of gravel, 160 parts of water, 4.2 parts of water reducer, 4.2 parts of urea, 0.0063 parts of plant urease and 3 to 8 parts of magnesium oxide.

[0013] Furthermore, the method for preparing the self-repairing concrete material comprises any one of the following:

[0014] Method 1, using the raw materials for preparing the first self-repairing concrete material, the preparation method comprises: mixing sand, gravel, cement, fly ash, mineral powder, urea and plant urease according to mass fractions to obtain a mixed system, then mixing a water reducer and water for a second time and adding the mixture to the mixed system, stirring evenly, to obtain the self-repairing concrete material;

[0015] Method 2, using the second self-repairing concrete material preparation raw materials, the preparation method includes: mixing sand, gravel, cement, fly ash, mineral powder, urea, plant urease and magnesium oxide according to mass fractions to obtain a mixed system, and then mixing the water reducer and water for a second time and adding them to the mixed system, stirring evenly, to obtain the concrete material.

[0016] Furthermore, the time for the first mixing is 2 minutes, the time for the second mixing is 20 seconds, and the time for the stirring is 2 to 5 minutes.

[0017] Adding a certain proportion of urea and urease to concrete can induce the formation of calcium carbonate crystals with good cementing properties. Such crystals can cement loose sand particles to form a strong structure and automatically repair concrete cracks from the inside. In addition, the addition of magnesium oxide (active magnesium oxide) can also repair cracks and improve concrete performance. Magnesium oxide has the characteristic of delayed expansion. When it comes into contact with water, it converts chemical energy into mechanical energy, limits the expansion of concrete, and reduces the formation of cracks. In addition, the self-healing time of magnesium oxide-modified concrete will be extended, and some shrinkage cracks can be effectively repaired in the early stages of maintenance. Therefore, the simultaneous use of urease-induced calcium carbonate precipitation technology and the modification effect of magnesium oxide can greatly improve the self-healing ability of concrete.

[0018] The present invention discloses the following technical effects:

[0019] (1) The plant urease of the present invention can hydrolyze urea to generate CO2, which will be converted into CO3 under alkaline conditions. 2- , then CO3 2- Will react with Ca in the environment 2+ Reaction, forming calcium carbonate precipitation at the cracks, greatly improving the waterproof and anti-seepage effects, meeting the needs of the project and improving the quality of the project.

[0020] (2) As cement hydration proceeds, the plant urease and magnesium oxide of the present invention gradually take effect. Under alkaline conditions, urease catalyzes the hydrolysis of urea to produce CO3 2- ,CO3 2- Ca in the environment 2+ The reaction generates calcium carbonate precipitation with good gelling properties at the cracks. Magnesium oxide can delay expansion when concrete shrinks and cracks, effectively reducing the generation of early cracks and prolonging the self-healing time of concrete. The synergistic effect of the two greatly reduces the generation of cracks, improves the self-healing ability of concrete, and the performance test can meet the needs of the project, which can undoubtedly greatly improve the quality of the project.

[0021] (3) Adding the admixture of the present invention can improve the anti-seepage ability of the self-repairing concrete material, so that the waterproof and anti-seepage effects of the material meet the engineering requirements and improve the engineering quality.

[0022] (4) The self-repairing concrete material of the present invention combines urease-induced calcium carbonate precipitation technology and magnesium oxide-modified concrete technology, and its self-healing ability is greatly improved. It has good compactness, waterproofness and impermeability. In addition, its preparation method is simple and low-cost. While improving the waterproof and impermeability performance, it can complete the construction without affecting its workability and strength performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a microstructure diagram of the self-repairing concrete material prepared in Example 1 of the present invention;

[0025] Figure 2 This is a microstructure diagram of the self-repairing concrete material prepared in Example 2 of the present invention;

[0026] Figure 3 This is a microstructure diagram of the blank concrete prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] The “parts” described in the following examples are all “parts by mass”.

[0033] The content of plant urease in the watermelon seeds used in the following examples of the present invention is about 0.15 wt.%.

[0034] The cement used in the following examples and comparative examples of the present invention is ordinary Portland cement with a grade of 42.5; the sand used in the following examples of the present invention is medium sand, the particle size of the gravel is 5 to 20 mm, the fly ash is Class II fly ash, and the mineral powder is S95 mineral powder.

[0035] Example 1

[0036] A method for preparing a self-repairing concrete material:

[0037] (1) 728 parts of sand, 728 parts of gravel, 320 parts of cement, 60 parts of fly ash, 40 parts of mineral powder, 4.2 parts of urea and 4.2 parts of watermelon seeds (powdered, containing 0.0063 parts of plant urease) were mixed for 2 minutes to obtain a mixed system A.

[0038] (2) 4.2 parts of water reducer and 160 parts of water were mixed for 20 seconds, added to the mixed system A within 25 seconds, and stirred at room temperature for 3 minutes to obtain a self-repairing concrete material (C40 guardrail concrete with a bulk density of 2400 kg / m 3 , water-cement ratio 0.38, sand rate 40%).

[0039] Example 2

[0040] A method for preparing a self-repairing concrete material:

[0041] (1) 728 parts of sand, 728 parts of gravel, 320 parts of cement, 60 parts of fly ash, 40 parts of mineral powder, 4.2 parts of urea, 4.2 parts of watermelon seeds (powdered, containing 0.0063 parts of plant urease) and 5 parts of magnesium oxide were mixed for 2 minutes to obtain a mixed system A.

[0042] (2) 4.2 parts of water reducer and 160 parts of water were mixed for 20 seconds, added to the mixed system A within 25 seconds, and stirred at room temperature for 3 minutes to obtain a self-repairing concrete material (C40 guardrail concrete with a bulk density of 2400 kg / m 3 , water-cement ratio 0.38, sand rate 40%).

[0043] Comparative Example 1

[0044] Preparation of blank concrete:

[0045] (1) 728 parts of sand, 728 parts of gravel, 320 parts of cement, 60 parts of fly ash and 40 parts of mineral powder were mixed for 2 minutes to obtain a mixed system A.

[0046] (2) 4.2 parts of water reducer and 160 parts of water were mixed for 20 seconds, added to the mixed system A within 25 seconds, and stirred at room temperature for 3 minutes to obtain blank concrete.

[0047] The properties of the concrete prepared in Examples 1 to 2 of the present invention and Comparative Example 1 were measured, and the results are shown in Table 1.

[0048] The standards for performance measurement are: GB / T50080-2016 Standard for test methods for performance of ordinary concrete mixtures; GB / T50081-2019 Standard for test methods for physical and mechanical properties of concrete.

[0049] Table 1

[0050]

[0051] The internal structure of the 7-day-old mortar block prepared by the concrete of Comparative Example 1 of the present invention is loose and porous, and not dense ( Figure 3 ); The pores of the concrete block with a 7-day age prepared by the self-repairing concrete material of Example 1 of the present invention are significantly reduced, indicating that the internal structure of the self-repairing concrete block is more compact. This is because the interior of the self-repairing concrete is a highly alkaline environment with a pH value of 12 to 13. The urease released by the watermelon seeds hydrolyzes urea to generate CO2. The alkaline conditions can further convert CO2 into carbonate ions, which then react with the Ca in the surrounding solution to form a carbonyl ion. 2+ The reaction generates calcium carbonate precipitation, which fills the pores inside the concrete test block, making the pores smaller and the structure of the formed test block denser ( Figure 1 ).

[0052] In the early stage of the self-repairing concrete material containing watermelon seeds of the present invention, as the cement hydration proceeds, the watermelon seeds gradually take effect, secrete urease, and urease hydrolyzes urea to generate CO2, which will be converted into CO3 under alkaline conditions. 2- , then CO3 2- Will react with Ca in the environment 2+ The self-repairing concrete material of the present invention can greatly improve the waterproof and anti-seepage effects, meet the needs of the project, and improve the quality of the project.

[0053] The pores of the 7-day-old test block prepared by the self-repairing concrete material of Example 2 of the present invention are significantly reduced, indicating that the internal structure of the test block cast by the self-repairing concrete is more compact, which is due to the application of urease-induced calcium carbonate precipitation and magnesium oxide-modified concrete synergistic technology in this system. In the concrete of a highly alkaline environment (pH 12-13), the urease released by watermelon seeds catalyzes the hydrolysis of urea to generate CO3 2- ,CO3 2- With the surrounding solution Ca 2+ The reaction generates calcium carbonate precipitation, which then fills the pores inside the concrete specimen, making the pores smaller ( Figure 2 ). Magnesium oxide can delay the expansion of concrete shrinkage cracks, effectively reduce the occurrence of early cracks, and prolong the self-healing time of concrete. Therefore, due to the synergistic effect of these two aspects, the structure of the concrete specimen after molding is denser.

[0054] In the early stage of the self-repairing concrete material containing watermelon seeds and magnesium oxide, as the cement hydration proceeds, the urease and magnesium oxide secreted by the watermelon seeds gradually take effect. Under alkaline conditions, urease catalyzes the hydrolysis of urea to produce CO3 2- ,CO3 2- Ca in the environment 2+The reaction generates calcium carbonate precipitation with good gelling properties at the cracks. Magnesium oxide can delay expansion when concrete shrinks and cracks, effectively reducing the generation of early cracks and prolonging the self-healing time of concrete. The synergistic effect of the two greatly reduces the generation of cracks, improves the self-healing ability of concrete, and the performance test can meet the needs of the project, which can undoubtedly greatly improve the quality of the project.

[0055] Effect Example 2

[0056] According to GB / T50082-2009 standard for long-term performance and durability test of ordinary concrete, the concrete prepared in Examples 1 to 2 and Comparative Example 1 was tested for its impermeability.

[0057] The test method is as follows: weigh 20L40 guardrail concrete according to the mix ratio, mix it with a test mixer, test the slump, air content and other indicators, and then form a group of 3 anti-seepage test blocks (brush with water-based release agent); demold after 1 day, use a wire brush to brush off the cement slurry film on both end surfaces, and then send it to the standard curing room for curing; take it out on the 14th day for anti-seepage performance test.

[0058] Table 2 Anti-seepage performance

[0059] Test No. Water seepage height / mm Comparative Example 1 32.8 Example 1 29.2 Example 2 25.7

[0060] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A self-repairing concrete material, characterized in that: The invention is composed of the following raw materials in parts by mass: 320 parts of cement, 60 parts of fly ash, 40 parts of mineral powder, 728 parts of sand, 1092 parts of gravel, 160 parts of water, 4.2 parts of water reducing agent, 4.2 parts of urea, 0.0063 parts of plant urease and 3-8 parts of magnesium oxide.

2. The self-repairing concrete material according to claim 1, characterized in that: The method for preparing the self-repairing concrete material comprises the following steps: Sand, gravel, cement, fly ash, mineral powder, urea, plant urease and magnesium oxide are mixed once according to mass proportions to obtain a mixed system, and then a water reducer and water are mixed twice and added to the mixed system, and stirred evenly to obtain the concrete material.

3. The self-repairing concrete material according to claim 2, characterized in that: The time for the first mixing is 2 minutes, the time for the second mixing is 20 seconds; and the time for the stirring is 2 to 5 minutes.

Citation Information

Cited By

  • Composite additive for self-repairing concrete as well as preparation method and application of composite additive

    CN119797802A

  • Rock mass pore network reconstruction method based on urease induced calcium carbonate solidification