A method for sealing the end face of a movable guide vane of a water turbine
By arranging a steel structure skeleton in the sealing groove of the turbine's movable guide vane and using vacuum and high-pressure casting of polyurethane material, the problem of insufficient bonding force of the sealing strip was solved, and the sealing performance was improved and the reliability of the unit operation was enhanced.
Patent Information
- Application Number
- CN202311005943.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-08-10
AI Technical Summary
The combined force between the sealing strip and the sealing groove of the movable guide vane of the turbine is insufficient, resulting in loose sealing, easy detachment, short service life, difficulty in shutting down the unit and problems of creeping.
A steel structure skeleton is set up in the sealing groove, and a sealing strip is formed by pouring polyurethane material under vacuum and high pressure. Combining the physical combination of the steel structure skeleton and the chemical bonding of polyurethane, the bonding force between the sealing strip and the sealing groove is enhanced to prevent the sealing strip from detaching.
Significantly improves the bonding force between the sealing strip and the sealing groove, preventing the sealing strip from being scraped off or eroded, ensuring good sealing performance, reducing water energy waste, and improving power generation efficiency and unit operation reliability.
Smart Images

Figure CN116838519B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water turbine movable guide vane sealing, and in particular relates to a water turbine movable guide vane end face sealing method. Background Art
[0002] The water guide mechanism of the turbine is an important component to ensure the stable operation of the unit of the hydropower station. The movable guide vane is a key device used to guide and cut off the water flow of the turbine and regulate the flow rate of water through the turbine. The movable guide vane end face seal is installed on the top cover and the bottom ring, and is used for the movable guide vane of the turbine to stop water when cutting off the water flow. When the turbine is shut down and the movable guide vane is closed, the sealing strips on the upper and lower end faces and the vertical surface of the movable guide vane play a sealing role, on the one hand, preventing the loss of water energy in the pressure volute, and on the other hand, preventing the unit from creeping in the shutdown state. The movable guide vane seal of the turbine has the form of hard seal, soft seal, and a combination of hard and soft.
[0003] In the early days of domestic hydropower station turbine movable guide vane sealing, oil-resistant rubber strips were installed in the dovetail groove for sealing. When sealed in this way, the bonding force between the rubber strip and the dovetail groove was insufficient. In addition, after years of operation, the dovetail groove was prone to abrasion and corrosion damage, resulting in irregular damage to the dovetail groove, which would lead to reduced fixing force of the rubber strip and poor sealing. The rubber strip therefore had the disadvantages of being easy to fall off and having a short service life. It would also lead to large gaps on the end faces of the guide vanes of the unit and increased water leakage from the movable guide vanes, causing difficulties in shutting down the unit and creeping after shutdown.
[0004] At present, the movable guide vane seal is mostly improved by changing the sealing structure, changing the dovetail groove to a pressure plate seal, or replacing the seat ring with stainless steel. However, for some turbines, the seat ring is not suitable for disassembly and machining, and cannot be changed to a pressure plate seal. In addition, repairing the dovetail groove with abrasion and damage is time-consuming, labor-intensive, and costly. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a method for sealing the end face of a movable guide vane of a water turbine, which improves the bonding force between a sealing strip and a sealing groove.
[0006] Based on the above purpose, the present invention is achieved through the following technical solutions:
[0007] A method for sealing the end face of a movable guide vane of a water turbine comprises the following steps:
[0008] S1: pre-treat the sealing groove;
[0009] S2: A steel structure frame is set in the upper part of the sealing groove, the sealing groove is sandblasted again, and then the mold is installed and the periphery of the mold is sealed with glue;
[0010] The steel structure frame divides the sealing strip in the sealing groove into two parts. The steel structure frame in the middle and upper part of the sealing groove can ensure that the volume of the sealing strip under the steel structure frame is larger, thereby ensuring the bonding force between the sealing strip and the sealing groove, and preventing the sealing strip from being deformed or separated from the sealing groove when being eroded by the movable guide vane of the turbine or high-speed water flow;
[0011] When the colloid is poured, it can flow into the bottom of the sealing groove through the metal mesh pores of the steel structure frame. After the colloid is solidified, the sealing strip cast by the colloid can achieve physical combination with the steel structure frame, effectively preventing the sealing strip from separating from the sealing groove; the sandblasting treatment can remove welding slag and rust on the steel structure frame, and prevent the cast sealing strip from separating from the sealing groove and the steel structure frame; the glue can seal the mold to prevent the overflow of the colloid. The glue can also fix the mold to prevent the mold from separating from the sealing groove during the pouring process;
[0012] S3: Casting polyurethane: Mix the polyurethane prepolymer and the chain extender to form a colloid, pour the colloid into a pressure tank, and then use high-pressure gas to inject the colloid into the sealing groove fixed with the mold, and keep it warm and solidify; the gas pressure is less than 0.2MPa;
[0013] The colloid after the polyurethane prepolymer and the chain extender are evenly fused can enhance the bonding strength between the colloid and the sealing groove, increase the chemical bonding of the rubber strip, and use vacuum high-pressure casting technology to cast the wear-resistant and tear-resistant polyurethane material into a sealing strip in the sealing groove. The colloid is injected into the sealing groove fixed with the mold by high-pressure gas, which is convenient for exhausting the air in the sealing groove fixed with the mold, and also convenient for the colloid to quickly fill the sealing groove fixed with the mold, so as to prevent the molding of the rubber strip during the injection process and affect the quality of the cast sealing strip;
[0014] The temperature and pouring pressure of the colloid can make the formed sealing strip tightly fixed in the sealing groove, effectively guarantee the bonding force between the sealing strip and the sealing groove, and avoid the directly installed sealing strip being easily scraped off by the movable guide vane or eroded by high-speed water flow; ensure that a higher temperature is reached, and the rubber strip in the mold is cured and formed by the electric heating pad, and the insulation material is used to make the rubber strip evenly cured at a higher temperature;
[0015] S4: After curing, the flash of the cast sealing strip is cut off, and the surrounding cement is removed, and the sealing strip is formed by heating and vulcanizing at 100-130℃ for 12 hours, that is, the sealing of the end face of the turbine movable guide vane is completed. Heating and vulcanizing the sealing strip can promote the sealing strip to achieve better performance.
[0016] Preferably, the specific process of heat preservation curing is: firstly curing at 100-120° C. for 2-4 h, and then curing at 70-90° C. for 6-8 h.
[0017] Preferably, the polyurethane prepolymer contains alkylamine functionalized graphene oxide.
[0018] Preferably, the steel structure skeleton is a steel plate mesh.
[0019] Preferably, the specific process of pretreatment in step S1 is: chisel off the mortar coating within 5-10 cm on both sides of the sealing groove, grind the inside of the sealing groove with an angle grinder after chiseling off, and then use a sandblasting gun to remove rust and stains in the sealing groove, and the sealing groove is exposed after cleaning. If the chiseling range is less than 5 cm, the external dirt will easily enter the sealing groove, and if the chiseling range is greater than 10 cm, it will increase the difficulty of construction and affect the construction efficiency; sandblasting can effectively remove all dirt in the sealing groove, which is conducive to the close combination of the cast sealing strip and the sealing groove.
[0020] Preferably, in step S4, after the vulcanization is completed, a lubricating material is coated on the surface of the sealing strip, which can play a lubricating role in the later movable guide vane closing test of the turbine and prevent the surface of the sealing strip from being scratched.
[0021] Preferably, the sealing strip comprises a dovetail bottom plate whose bottom matches the sealing groove, a curved convex strip at the top of the dovetail bottom plate, and two sides of the curved convex strip are connected to two sides of the top of the sealing groove; a steel structure frame is provided inside the dovetail bottom plate.
[0022] Preferably, the sealing groove is a dovetail groove, a steel structure frame is horizontally arranged in the sealing groove, the steel structure frame is a steel plate mesh, and the steel structure frame is horizontally arranged in the upper middle part of the sealing groove; mold grooves are opened on both sides of the sealing groove.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Through the treatment of the turbine movable guide vane end face sealing method, a polyurethane sealing strip with good sealing performance, excellent wear resistance and excellent erosion resistance can be obtained. The sealing strip and the sealing groove are not only chemically bonded, but also physically bonded by the welded steel plate mesh, thereby effectively improving the bonding force between the sealing strip and the sealing groove, and can effectively solve the problem that the sealing strip directly installed in the sealing groove is easily scraped off by the movable guide vane or eroded by high-speed water flow.
[0025] (2) The present invention utilizes vacuum high-pressure casting technology to cast wear-resistant and tear-resistant polyurethane material into a sealing strip. The size of the sealing strip is determined by the actual size of the sealing groove. The sealing groove can be of regular shape or of irregular shape after being damaged by water erosion. The damaged part of the sealing groove can be filled with polyurethane to restore the designed size. The protruding height of the sealing strip of the present invention is controlled by a customized mold, which is processed according to the original designed size of the sealing groove. The sealing strip of the present invention has a strong bonding force with the sealing groove, which is ensured by the high-strength adhesive and the steel structure skeleton design.
[0026] (3) The present invention can divide the sealing groove into an upper and lower part by welding a steel structure frame at the middle and upper part of the sealing groove, and then use vacuum high-pressure casting technology to cast colloid into the mold and the sealing groove. The colloid passes through the steel structure frame and is cast into the sealing groove. The sealing strip formed by the colloid casting is physically combined with the steel structure frame to prevent the sealing strip from being separated from the sealing groove. The colloid formed by the uniform fusion of the polyurethane prepolymer and the chain extender can increase the chemical adhesion of the colloid, increase the bonding strength between the sealing strip formed by the colloid and the sealing groove, and realize a double combination of chemical bonding and physical bonding between the sealing strip and the sealing groove profile, effectively improving the bonding force between the sealing strip and the sealing groove, preventing the sealing strip from falling off, and ensuring the excellent sealing effect of the sealing strip, thereby reducing the waste of water energy when the movable guide vane end face is sealed, increasing the power generation efficiency, and improving the overall operation reliability of the unit. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a schematic cross-sectional view of the sealing strip in Example 1;
[0028] Figure 2 is a top view of the sealing strip in Example 1;
[0029] Figure 3 is a schematic diagram of the process of Example 1;
[0030] Figure 4 It is a schematic diagram of the construction effect of the present invention in Example 1;
[0031] Figure 5 It is a schematic diagram of the process of Example 2.
[0032] In the figure, there are sealing groove 1, steel structure frame 2, sealing strip 3, mold 4, and mortar coating 5. DETAILED DESCRIPTION
[0033] The present invention is further described below by means of specific examples, but the scope of the present invention is not limited thereto.
[0034] Example 1
[0035] A method for sealing the end face of a movable guide vane of a water turbine, the process of which is as follows: Figure 3 As shown, the following steps are included:
[0036] S1: pre-treat the sealing groove 1; the specific process of the pre-treatment is: chisel off the mortar coating 5 within 5-10 cm on both sides of the sealing groove 1, and then grind the sealing groove 1 with an angle grinder. The mortar at both ends of the sealing groove 1 needs to be cleaned to avoid affecting the fit of the mold 4 during installation, and then use a sandblasting gun to sandblast away the rust and stains in the sealing groove 1. After cleaning, the metallic luster is exposed in the sealing groove 1.
[0037] S2: Weld the steel structure frame 2 to the upper part of the sealing groove 1, sandblast the sealing groove 1 again, then install the mold 4, and seal the periphery of the mold 4 with glue; the steel structure frame 2 is a steel plate mesh.
[0038] The steel structure skeleton 2 divides the sealing strip 3 in the sealing groove 1 into two parts. The steel structure skeleton 2 in the middle and upper part of the sealing groove 1 can ensure that the volume of the sealing strip 3 under the steel structure skeleton 2 is larger, thereby ensuring the bonding force between the sealing strip 3 and the sealing groove 1 and preventing the sealing strip 3 from being deformed or separated from the sealing groove 1 when being eroded by the movable guide vanes of the turbine or the high-speed water flow.
[0039] When the colloid is poured, it can flow into the bottom of the sealing groove 1 through the metal mesh pores of the steel structure skeleton 2. After the colloid is solidified, the sealing strip 3 cast by the colloid can achieve physical combination with the steel structure skeleton 2, effectively preventing the sealing strip 3 from separating from the sealing groove 1; sandblasting again can remove welding slag and rust on the steel structure skeleton 2, and prevent the cast sealing strip 3 from being separated from the sealing groove 1 and the steel structure skeleton 2 during casting; the glue can seal the mold 4 to prevent the colloid from overflowing. The glue can also fix the mold 4 to prevent the mold 4 from separating from the sealing groove 1 during the pouring process.
[0040] S3: Casting polyurethane: Mix the polyurethane prepolymer and the chain extender to form a colloid, pour the colloid into a pressure tank, and then use high-pressure gas to inject the colloid into the sealing groove 1 fixed with the mold 4, and heat-insulate and cure; the gas pressure is less than 0.2MPa; the specific process of heat-insulating and curing is: first cure at 120°C for 2 hours, and then cure at 90°C for 6 hours; the polyurethane prepolymer contains alkylamine-functionalized graphene oxide.
[0041] The colloid formed by uniform fusion of the polyurethane prepolymer and the chain extender can enhance the bonding strength between the colloid and the sealing groove 1 and increase the chemical bonding of the rubber strip. The wear-resistant and tear-resistant polyurethane material is cast into the sealing groove 1 into a sealing strip 3 by using vacuum high-pressure casting technology. The colloid is injected into the sealing groove 1 fixed with the mold 4 by high-pressure gas, which facilitates the discharge of air in the sealing groove 1 fixed with the mold 4 and facilitates the rapid filling of the sealing groove 1 fixed with the mold 4 by the colloid, thereby preventing the molding of the rubber strip during the injection process from affecting the quality of the cast sealing strip 3.
[0042] The temperature of the colloid and the pouring pressure can make the formed sealing strip 3 tightly fixed in the sealing groove 1, effectively ensure the bonding force between the sealing strip 3 and the sealing groove 1, and avoid the directly installed sealing strip 3 being easily scraped off by the movable guide vane or eroded by high-speed water flow; the thermal insulation curing ensures that a higher temperature is reached, and the rubber strip in the mold 4 is cured and formed by the electric heating pad, and the thermal insulation material is used to enable the rubber strip to achieve uniform curing at a higher temperature.
[0043] S4: After the curing is completed, the mold 4 is removed, the flash of the cast sealing strip 3 is cut off, and the surrounding cement is removed. The sealing strip 3 is formed by heating and vulcanizing at 120°C for 12 hours, that is, the sealing of the end face of the active guide vane of the turbine is completed; after the vulcanization is completed, the lubricating material is coated on the surface of the sealing strip 3. The construction effect of the sealing of the end face of the active guide vane of the turbine is as follows: Figure 4 The sealing strip 3 includes a dovetail bottom plate with a bottom that matches the sealing groove, an arc-shaped convex strip on the top of the dovetail bottom plate, and the two sides of the arc-shaped convex strip are connected to the two sides of the top of the sealing groove; the dovetail bottom plate has a steel structure frame 2. The structure of the cast sealing strip 3 is as follows Figure 1-2 shown.
[0044] Example 2
[0045] A method for sealing the end face of a movable guide vane of a water turbine, the process of which is as follows: Figure 5 As shown, the following steps are included:
[0046] S1: pre-treating the sealing groove 1;
[0047] S2: a steel structure frame 2 is arranged in the upper part of the sealing groove 1, the sealing groove 1 is sandblasted again, and then the mold 4 is installed, and the periphery of the mold 4 is sealed with glue;
[0048] The steel structure frame 2 divides the sealing strip 3 in the sealing groove 1 into two parts. The steel structure frame 2 in the middle and upper part of the sealing groove 1 can ensure that the volume of the sealing strip 3 under the steel structure frame 2 is larger, thereby ensuring the bonding force between the sealing strip 3 and the sealing groove 1, and preventing the sealing strip 3 from being deformed or separated from the sealing groove 1 when being eroded by the movable guide vane of the turbine or the high-speed water flow;
[0049] When the colloid is poured, it can flow into the bottom of the sealing groove 1 through the metal mesh pores of the steel structure skeleton 2. After the colloid is solidified, the sealing strip 3 cast by the colloid can achieve physical combination with the steel structure skeleton 2, effectively preventing the sealing strip 3 from being separated from the sealing groove 1; the sandblasting treatment can remove the welding slag and the rust of the steel structure skeleton 2, and prevent the cast sealing strip 3 from being separated from the sealing groove 1 and the steel structure skeleton 2; the glue can seal the mold 4 to prevent the overflow of the colloid, and the glue can also fix the mold 4 to prevent the mold 4 from being separated from the sealing groove 1 during the pouring process;
[0050] S3: Casting polyurethane: The polyurethane prepolymer and the chain extender are mixed and fused to form a colloid, the colloid is poured into a pressure tank, and then the colloid is injected into the sealing groove 1 fixed with the mold 4 by high-pressure gas, and is heat-insulated and cured; the gas pressure is less than 0.2MPa;
[0051] The colloid after the polyurethane prepolymer and the chain extender are evenly fused can enhance the bonding strength between the colloid and the sealing groove 1, increase the chemical bonding of the rubber strip, and use vacuum high-pressure casting technology to cast the wear-resistant and tear-resistant polyurethane material into the sealing groove 1 to form a sealing strip 3. The colloid is injected into the sealing groove 1 fixed with the mold 4 by high-pressure gas, which is convenient for exhausting the air in the sealing groove 1 fixed with the mold 4, and also convenient for the colloid to quickly fill the sealing groove 1 fixed with the mold 4, so as to prevent the molding of the rubber strip during the injection process from affecting the quality of the cast sealing strip 3;
[0052] The temperature and pouring pressure of the colloid can make the formed sealing strip 3 tightly fixed in the sealing groove 1, effectively guarantee the bonding force between the sealing strip 3 and the sealing groove 1, and avoid the situation that the directly installed sealing strip 3 is easily scraped off by the movable guide vane or eroded by the high-speed water flow; ensure that a higher temperature is reached, and the rubber strip in the mold 4 is cured and formed by the electric heating pad, and the insulation material is used to make the rubber strip evenly cured at a higher temperature;
[0053] S4: After curing, the flash of the cast sealing strip 3 is cut off, and the surrounding cement is removed, and the sealing strip 3 is formed by heating and vulcanizing at 100-130°C for 12 hours, that is, the sealing of the end face of the turbine movable guide vane is completed. The heating and vulcanization of the sealing strip 3 can promote the sealing strip 3 to achieve better performance.
[0054] Example 3
[0055] A method for sealing the end face of a movable guide vane of a water turbine is different from that of Example 1 in that: the specific process of heat preservation and curing in step S3 is: first curing at 100° C. for 4 hours, and then curing at 70° C. for 8 hours.
[0056] Example 4
[0057] A method for sealing the end face of a movable guide vane of a water turbine is different from that of Example 1 in that the gas pressure in step S3 is 0.2 MPa.
[0058] Example 5
[0059] A method for sealing the end face of a movable guide vane of a water turbine is different from that of Embodiment 1 in that: the gas pressure in step S3 is 0.1 MPa.
[0060] Example 6
[0061] A method for sealing the end face of a movable guide vane of a water turbine, which is different from Example 1 in that: the gas pressure in step S3 is 0.05 MPa.
[0062] Example 7
[0063] A sealing strip for the end face of a movable guide vane of a water turbine, wherein the bottom of the sealing strip 3 is a dovetail-like bottom plate matched with a sealing groove 1, the top of the dovetail-like bottom plate is provided with an arc-shaped convex strip, and the two sides of the arc-shaped convex strip are connected to the two sides of the top of the sealing groove 1; a steel structure frame 2 is provided inside the dovetail-like bottom plate, and the steel structure frame 2 is a steel plate mesh.
[0064] Example 8
[0065] A sealing groove for the end face of a movable guide vane of a water turbine, wherein the sealing groove 1 is a dovetail groove, a steel structure frame 2 is horizontally arranged in the sealing groove 1, the steel structure frame 2 is a steel plate mesh, and the steel structure frame 2 is horizontally arranged in the middle and upper part of the sealing groove 1; mold grooves are opened on both sides of the sealing groove 1.
[0066] The above description is only a preferred embodiment of the present invention, but is not limited to the above examples. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for sealing the end face of a movable guide vane of a water turbine, characterized in that: The following steps are involved: S1: pre-treat the sealing groove; S2: Set a steel structure frame in the upper part of the sealing groove, and then install the mold; S3: Casting polyurethane: The polyurethane prepolymer and the chain extender are mixed and fused to form a colloid, and then the colloid is injected into a sealing groove fixed with a mold by high-pressure gas, and then cured by heat preservation; the gas pressure is less than 0.2MPa; S4: After curing, heat and vulcanize at 100-130℃ for 12 hours to form a sealing strip, thus completing the sealing of the end face of the turbine movable guide vane; The specific process of heat preservation curing is: firstly curing at 100-120°C for 2-4 hours, and then curing at 70-90°C for 6-8 hours; The polyurethane prepolymer contains alkylamine functionalized graphene oxide; The steel structure frame divides the sealing strip in the sealing groove into two parts. The steel structure frame in the middle and upper part of the sealing groove can ensure that the volume of the sealing strip under the steel structure frame is larger, thereby ensuring the bonding force between the sealing strip and the sealing groove, and preventing the sealing strip from being deformed or separated from the sealing groove when being eroded by the movable guide vane of the turbine or high-speed water flow; The specific process of the pretreatment in step S1 is: chiseling off the mortar coating within 5-10 cm on both sides of the sealing groove, and then grinding the sealing groove to remove rust and stains until the metallic luster is exposed; In step S4, after the vulcanization is completed, a lubricating material is applied to the surface of the sealing strip; The sealing strip comprises a dovetail bottom plate whose bottom matches the sealing groove, an arc-shaped convex strip is arranged at the top of the dovetail bottom plate, and two sides of the arc-shaped convex strip are connected to two sides of the top of the sealing groove; a steel structure frame is arranged inside the dovetail bottom plate.
2. The method for sealing the end face of a movable guide vane of a water turbine according to claim 1, characterized in that: The steel structure skeleton is a steel plate mesh.
Citation Information
Patent Citations
Synthetic method of thermocuring polyurethane elastomer composite material for sealing materials
CN105461877A
Steel-plastic composite polyurethane movable guide vane facade sealing device
CN105604768A
Shield segment sealing strip manufacturing method
CN110509489A
Manufacturing method of multi-layer multi-hardness polyurethane rubber core
CN112045914A
Hydropower station movable guide vane lower end face sealing groove machining method
CN116532988A