Binders for all-solid-state secondary batteries, binder compositions for all-solid-state secondary batteries, slurries for all-solid-state secondary batteries, solid electrolyte sheets for all-solid-state secondary batteries, and methods for manufacturing the same, as well as all-solid-state secondary batteries and methods for manufacturing the same.
By using a conjugated diene copolymer binder with specific energy storage elastic modulus and loss tangent, the problems of molding and winding process of all-solid secondary batteries were solved, the yield and lithium-ion conductivity of the batteries were improved, and excellent cycle life characteristics were achieved.
Patent Information
- Application Number
- CN202280012080.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-29
- Filing Date
- 2022-01-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-01-14
AI Technical Summary
All-solid-state secondary batteries suffer from poor formability, active material peeling, and reduced capacity during manufacturing. Furthermore, the binder is prone to powdering and cracking during the winding process, affecting the yield rate.
Using conjugated diene copolymers as binders, which have specific energy storage elastic modulus and loss tangent, and combining them with modifiers and liquid media, an all-solid binder composition for secondary batteries is formed, improving adhesion and flexibility.
It achieves high yield and excellent lithium-ion conductivity in all-solid-state secondary batteries, improving the cycle life characteristics and formability of the batteries.
Smart Images

Figure QLYQS_1 
Figure BDA0004361682420000031 
Figure BDA0004361682420000091
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive for all-solid-state secondary batteries, an adhesive composition for all-solid-state secondary batteries containing the adhesive, a slurry for all-solid-state secondary batteries containing the composition and a solid electrolyte, a solid electrolyte sheet for all-solid-state secondary batteries formed by coating and drying the slurry on a substrate, a method for manufacturing the same, and an all-solid-state secondary battery having the sheet, and a method for manufacturing the same. Background Technology
[0002] Lithium-ion secondary batteries, widely used in automotive power supplies and household batteries, mostly employ electrolytes. Currently, all-solid-state secondary batteries, where the electrolyte is replaced with a solid electrolyte, making all constituent materials solid, are under development as the ultimate battery that combines safety, high energy density, and long lifespan.
[0003] All-solid-state secondary batteries, using solid electrolytes exhibiting high ion conductivity, eliminate the risks of leakage and fire, resulting in excellent safety and reliability. Furthermore, all-solid-state secondary batteries are suitable for achieving high energy density through electrode stacking. Specifically, batteries can be fabricated with a structure consisting of an active material layer and a solid electrolyte layer arranged and connected in series. In this case, since the metal encapsulation for sealing the battery cells, the copper wires connecting the battery cells, and the busbars can be omitted, the energy density of the battery can be significantly increased. Additionally, good compatibility with high-potential cathode materials is another advantage.
[0004] On the other hand, challenges in manufacturing all-solid-state secondary batteries continue to emerge. Specifically, when a press-molded body is made by mixing the solid electrolyte (as the electrolyte) and the active material to increase the contact area, the press-molded body becomes hard, brittle, and lacks processability. In addition, the active material undergoes volume changes due to the adsorption and release of lithium ions, resulting in problems such as active material peeling off during charge-discharge cycles and a significant decrease in capacity in the aforementioned press-molded body.
[0005] Therefore, in order to improve moldability, techniques have been studied to further add binder components composed of polymeric compounds to the above mixture to improve moldability (for example, see Patent Documents 1-4).
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent Document 1: Japanese Patent Application Publication No. 11-86899
[0009] Patent Document 2: Japanese Patent Publication No. 7-87045
[0010] Patent Document 3: International Publication No. 2009 / 107784
[0011] Patent Document 4: Japanese Patent No. 5120522 Summary of the Invention
[0012] Due to improved formability, sheets containing solid electrolytes (sheets with a solid electrolyte layer and an electrode active material layer) can be manufactured from the previous single-sheet processing method to a high-productivity roll-to-roll method, and development for industrial production is underway.
[0013] However, when using conventional binders, powder shedding and cracking sometimes occur during the winding process of the sheet containing solid electrolyte, as well as the storage and transfer processes of the wound sheet containing solid electrolyte. This poses a risk of not obtaining an all-solid-state secondary battery with the desired performance and yield, requiring further improvement.
[0014] Some embodiments of the present invention provide an all-solid-state binder for secondary batteries that has excellent adhesion and flexibility while also exhibiting good cycle life characteristics and achieving high yield, and an all-solid-state binder composition containing the binder.
[0015] This invention was made to solve at least a part of the above-mentioned problems and can be implemented in any of the following ways.
[0016] One embodiment of the all-solid-state secondary battery binder of the present invention contains a conjugated diene copolymer (A).
[0017] The aforementioned conjugated diene copolymer (A) has aromatic vinyl units based on aromatic vinyl compounds and conjugated diene units based on conjugated diene compounds.
[0018] The storage modulus (G') measured using a dynamic viscoelasticity measuring device at a temperature of 25℃, a frequency of 0.1Hz, and a strain of 1% was 4.0 × 10⁻⁶. 4 Pa ~ 2.0 × 10 5 Pa and the loss tangent (tanδ) is 0.10 to 0.80.
[0019] In one embodiment of the binder for the aforementioned all-solid-state secondary batteries,
[0020] When the composition ratio (molar ratio) of the structural unit represented by the following formula (1), the following formula (2), the following formula (3) and the following formula (4) in the above conjugated diene copolymer (A) is set as p, q, r and s respectively, the value α represented by the following mathematical formula (i) can be less than 0.7.
[0021] α=(p+(0.5×r)) / (p+q+(0.5×r)+s)···(i)
[0022]
[0023] In any of the above-mentioned methods of binders for all-solid secondary batteries,
[0024] The bonded styrene content of the above-mentioned conjugated diene copolymer (A) can be 5% to 45%.
[0025] In any of the above-mentioned methods of binders for all-solid secondary batteries,
[0026] The conjugated diene copolymer (A) described above may have units based on a modifier containing at least one atom selected from nitrogen, oxygen, silicon, germanium and tin atoms.
[0027] One embodiment of the all-solid-state secondary battery binder composition of the present invention comprises an all-solid-state secondary battery binder of any of the above embodiments, and a liquid medium (B).
[0028] In one embodiment of the above-mentioned binder composition for all-solid-state secondary batteries,
[0029] The liquid medium (B) mentioned above can be at least one selected from aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, ketones, esters and ethers.
[0030] In any of the above-described binder compositions for all-solid-state secondary batteries,
[0031] The conjugated diene copolymer (A) described above can be dissolved in the liquid medium (B) described above.
[0032] One embodiment of the all-solid-state secondary battery slurry of the present invention comprises an all-solid-state secondary battery binder composition of any of the above embodiments, and a solid electrolyte.
[0033] In one embodiment of the above-mentioned slurry for all-solid-state secondary batteries,
[0034] The solid electrolyte may contain either a sulfide-based solid electrolyte or an oxide-based solid electrolyte.
[0035] One embodiment of the all-solid-state secondary battery of the present invention comprises at least a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer.
[0036] At least one of the above-mentioned positive electrode active material layer, the above-mentioned solid electrolyte layer and the above-mentioned negative electrode active material layer is a layer formed by coating and drying an all-solid secondary battery of any of the above-mentioned methods with a slurry.
[0037] One embodiment of the solid electrolyte sheet for all-solid-state secondary batteries of the present invention comprises a layer formed by coating a slurry for all-solid-state secondary batteries of any of the above embodiments onto a substrate and drying it.
[0038] One method for manufacturing a solid electrolyte sheet for an all-solid-state secondary battery according to the present invention includes a step of coating an all-solid-state secondary battery slurry of any of the above-described methods onto a substrate and drying it.
[0039] One method of manufacturing the all-solid-state secondary battery of the present invention is to manufacture the all-solid-state secondary battery by means of the method for manufacturing solid electrolyte sheets for all-solid-state secondary batteries described above.
[0040] The binder for all-solid-state secondary batteries according to the present invention, when used as a material for the solid electrolyte layer and / or active material layer of an all-solid-state secondary battery, can significantly improve adhesion and flexibility. As a result, since the formability during pressure molding becomes excellent, the following superior effects can be achieved: an all-solid-state secondary battery with excellent lithium-ion conductivity and good cycle life characteristics can be obtained, thereby enabling a high yield rate. Detailed Implementation
[0041] The preferred embodiments of the present invention will now be described in detail. It should be noted that the present invention is not limited to the embodiments described below, but also includes various modifications that can be implemented without changing the spirit of the invention. It should be noted that "(meth)acrylic acid" in this specification refers to both "acrylic acid" and "methacrylic acid".
[0042] In this specification, the numerical range described as “X~Y” can be interpreted as a range that includes the value X as the lower limit and the value Y as the upper limit.
[0043] 1. Adhesive for all-solid-state secondary batteries
[0044] One embodiment of the present invention provides an all-solid-state binder for secondary batteries containing a conjugated diene copolymer (A). The conjugated diene copolymer (A) has aromatic vinyl units based on aromatic vinyl compounds and conjugated diene units based on conjugated diene compounds. Using a dynamic viscoelasticity measuring device, the storage modulus (G') measured at a temperature of 25°C, a frequency of 0.1 Hz, and a strain of 1% is 4.0 × 10⁻⁶. 4 Pa ~ 2.0 × 10 5 Pa and the loss tangent (tanδ) is 0.10 to 0.80.
[0045] In addition to the aromatic vinyl units and the conjugated diene units described above, the conjugated diene copolymer (A) may also contain structural units based on other monomers that can be copolymerized with it. The arrangement order of the structural units in the conjugated diene copolymer (A) is not particularly limited. That is, the conjugated diene copolymer (A) can be a block copolymer or a random copolymer.
[0046] The following sections will describe the manufacturing method and physical properties of the conjugated diene copolymer (A).
[0047] 1.1. Method for manufacturing conjugated diene copolymer (A)
[0048] The conjugated diene copolymer (A) can be manufactured, for example, by a method comprising: a polymerization step of polymerizing an aromatic vinyl compound and a conjugated diene compound to obtain a conjugated diene copolymer with active ends (polymerization step), and a step of modifying the ends of the obtained conjugated diene copolymer (modification step). Additionally, a step of hydrogenating the conjugated diene copolymer may also be included (hydrogenation step). Specifically, it can be manufactured according to the method described in International Publication No. 2014 / 133097, by appropriately varying the molecular weight, the amount of aromatic vinyl compound, the content of ethylene bonds, the hydrogenation rate, the type of modifier, etc., in a manner suitable for the intended use. The method for manufacturing the conjugated diene copolymer (A) will be described in detail below.
[0049] <Polymerization Process>
[0050] The polymerization process is a process of polymerizing monomers containing aromatic vinyl compounds and conjugated diene compounds to obtain conjugated diene copolymers with active ends.
[0051] As a polymerization method for obtaining conjugated diene copolymers, solution polymerization, gas-phase polymerization, and bulk polymerization can be used, with solution polymerization being particularly preferred. Furthermore, as a polymerization form, batch polymerization and continuous polymerization can be used. When using solution polymerization, as a specific example of a polymerization method, one can exemplify a method in which monomers containing aromatic vinyl compounds and conjugated diene compounds are polymerized in an organic solvent in the presence of a polymerization initiator and, if necessary, a vinyl control agent (hereinafter also referred to as a "randomizer").
[0052] Examples of aromatic vinyl compounds include styrene, divinylbenzene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, N,N-dimethylaminoethylstyrene, and diphenylethylene. Among these, compounds selected from styrene and divinylbenzene are particularly preferred. It should be noted that aromatic vinyl compounds can be used alone or in combination of two or more.
[0053] As conjugated diene compounds, other conjugated diene compounds besides 1,3-butadiene can also be used. There are no particular limitations on such conjugated diene compounds as long as they can copolymerize with 1,3-butadiene and aromatic vinyl compounds; examples include isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. Among the conjugated diene compounds other than 1,3-butadiene, isoprene is preferred. It should be noted that one conjugated diene compound can be used alone or in combination of two or more.
[0054] The conjugated diene copolymer (A) obtained by the polymerization process can be a copolymer of 1,3-butadiene and an aromatic vinyl compound, or a copolymer of 1,3-butadiene and a conjugated diene compound other than 1,3-butadiene and an aromatic vinyl compound. From the perspective of high reactivity in anionic polymerization, the conjugated diene copolymer (A) is preferably a copolymer obtained using 1,3-butadiene and styrene.
[0055] In the conjugated diene copolymer obtained by the polymerization process, the content of aromatic vinyl compounds relative to the total amount of monomers used in the polymerization is preferably 5 to 45% by mass, more preferably 8 to 30% by mass, and particularly preferably 10 to 27% by mass. Furthermore, by keeping the content of aromatic vinyl compounds within the above range, the adhesion and flexibility of the electrode are sometimes improved. The monomers used in the manufacture of the conjugated diene copolymer before hydrogenation preferably contain 55 to 95% by mass of butadiene, 5 to 45% by mass of aromatic vinyl compounds, and 0 to 40% by mass of conjugated diene compounds other than butadiene. It is preferable that such a combination of amounts can achieve both adhesion and flexibility of the electrode.
[0056] During polymerization, monomers other than conjugated diene compounds and aromatic vinyl compounds can be used. Examples of other monomers include acrylonitrile, methyl methacrylate, and ethyl methacrylate. The amount of other monomers used relative to the total amount of monomers used in the polymerization is preferably 20% by mass or less, more preferably 18% by mass or less, and particularly preferably 15% by mass or less.
[0057] As polymerization initiators, at least one of alkali metal compounds and alkaline earth metal compounds can be used. Alkali metal compounds and alkaline earth metal compounds commonly used as initiators for anionic polymerization can be used, such as alkyl lithiums like methyl lithium, ethyl lithium, n-propyl lithium, n-butyl lithium, sec-butyl lithium, and tert-butyl lithium; 1,4-dilithium butane, phenyl lithium, stilbene lithium, naphthyl lithium, sodium naphthyl, potassium naphthyl, di-n-butylmagnesium, di-n-hexylmagnesium, potassium ethoxy, and calcium stearate. Lithium compounds are preferred.
[0058] Furthermore, the polymerization reaction can be carried out in the presence of a compound (hereinafter also referred to as "compound (R)") obtained by mixing at least one of the above-mentioned alkali metal compounds and alkaline earth metal compounds with a compound (hereinafter also referred to as "compound (C1)") into the polymerization initiation terminal. By carrying out polymerization in the presence of compound (R), functional groups that interact with current collectors, solid electrolytes, etc., can be introduced into the polymerization initiation terminal of the conjugated diene copolymer. It should be noted that in this specification, "interaction" refers to the formation of covalent bonds between molecules, or the formation of intermolecular forces weaker than covalent bonds (e.g., electromagnetic forces acting between molecules such as ion-dipole interactions, dipole-dipole interactions, hydrogen bonds, van der Waals forces, etc.). Additionally, "functional group that interacts with current collectors, solid electrolytes, etc." refers to a group having at least one atom such as a nitrogen atom, an oxygen atom, a silicon atom, a sulfur atom, or a phosphorus atom.
[0059] As for the aforementioned compound (C1), there are no particular limitations as long as it has a partial structure in which nitrogen, oxygen, silicon, sulfur, and phosphorus atoms are directly bonded to hydrogen atoms. For example, nitrogen-containing compounds such as secondary amines, compounds containing hydroxyl groups, silicon-containing compounds such as tertiary silanes, compounds containing thiol groups, and compounds such as secondary phosphine can be used as the aforementioned compound (C1). Among these, nitrogen-containing compounds such as secondary amines are preferred. Specific examples of such nitrogen-containing compounds include dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, dioctylamine, dodecylmethyleneimine, N,N'-dimethyl-N'-trimethylsilyl-1,6-diaminohexane, piperidine, 3,3-dimethylpiperidine, 2,6-dimethylpiperidine, 1-methyl-4-(methylamino)piperidine, 2,2,6,6-tetramethylpiperidine, pyrrolidine, piperazine, 2,6-dimethylpiperazine, 1-ethylpiperazine, and 2-methylpiperazine. 1-Benzylpiperazine, 2,6-dimethylmorpholine, hexamethyleneimine, heptamethyleneimine, dicyclohexylamine, N-methylbenzylamine, di(2-ethylhexyl)amine, diallylamine, morpholine, N-(trimethylsilyl)piperazine, N-(tert-butyldimethylsilyl)piperazine, N'-[2-N,N-bis(trimethylsilyl)aminoethyl]piperazine, 1,3-bis(trimethylsilyl)-1,3,5-triazine, 5-benzyloxyindole, 3-azaspirocyclo[5,5]undecane, etc.
[0060] As the aforementioned compound (R), it is preferably the reaction product of a lithium compound such as alkyllithium and compound (C1). It should be noted that when polymerization is carried out in the presence of compound (R), compound (R) can be prepared by pre-mixing an alkali metal compound or an alkaline earth metal compound with compound (C1), and then adding the prepared compound (R) to the polymerization system for polymerization. Alternatively, compound (R) can be prepared by adding an alkali metal compound or an alkaline earth metal compound and compound (C1) to the polymerization system, mixing them in the polymerization system, and then carrying out polymerization.
[0061] Atactic agents can be used to adjust the content of ethylene bonds (1,2-ethylene bond content), etc. Examples of atactic agents include dimethoxybenzene, tetrahydrofuran, dimethoxyethane, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dibutyl ether, diethylene glycol dimethyl ether, 2,2-bis(tetrahydrofuranyl)propane, 2-(2-ethoxyethoxy)-2-methylpropane, triethylamine, pyridine, N-methylmorpholine, tetramethylethylenediamine, etc. These can be used alone or in combination of two or more.
[0062] As an organic solvent used in the polymerization, any organic solvent that is inactive in the reaction can be used, such as aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons. Hydrocarbons with 3 to 8 carbon atoms are preferred, and specific examples include n-pentane, isopentane, n-hexane, n-heptane, cyclohexane, propylene, 1-butene, isobutene, trans-2-butene, cis-2-butene, 1-pentyne, 2-pentyne, 1-hexene, 2-hexene, benzene, toluene, xylene, ethylbenzene, cyclopentane, methylcyclopentane, methylcyclohexane, 1-pentene, 2-pentene, and cyclohexene. It should be noted that one or more organic solvents can be used alone or in combination.
[0063] When using solution polymerization, considering the balance between productivity and ease of controlling the polymerization, the monomer concentration in the reaction solvent is preferably 5-50% by mass, more preferably 10-30% by mass. The polymerization temperature is preferably -20 to 150°C, more preferably 0-120°C, and particularly preferably 20-100°C. Furthermore, the polymerization reaction is preferably carried out at a pressure sufficient to substantially retain the monomer in the liquid phase. Such pressure can be obtained by methods such as pressurizing a gas that is inactive in the polymerization reaction within the reactor.
[0064] Regarding the conjugated diene copolymer obtained from the above polymerization, the content of 1,2-ethylene bonds in the structural units derived from butadiene is preferably 5 to 70% by mass, more preferably 10 to 65% by mass, and particularly preferably 20 to 60% by mass. If the 1,2-ethylene bond content is 5% by mass or more, there is a tendency for increased adhesion; if it is 70% by mass or less, there is a tendency for improved lithium-ion conductivity and cycle life characteristics. It should be noted that the 1,2-ethylene bond content is determined by... 1 The value was determined by H-NMR.
[0065] The unhydrogenated conjugated diene copolymer preferably has a random copolymer portion having structural units derived from butadiene and structural units derived from aromatic vinyl compounds. It is preferred in that it allows for better dispersibility of the active material and solid electrolyte by having such a specific random copolymer portion.
[0066] <Modification Process>
[0067] The modification process involves reacting the active ends of the conjugated diene copolymer obtained from the polymerization process with a compound (hereinafter also referred to as "compound (C2)") that introduces functional groups that interact with current collectors, solid electrolytes, etc., into the polymerization termination ends. This process can introduce functional groups that interact with current collectors, solid electrolytes, etc., into the polymerization termination ends of the conjugated diene copolymer. It should be noted that, in this specification, an active end refers to a portion (more specifically, a carboanion) existing at one end of the molecular chain, originating from a monomer having a carbon-carbon double bond and located outside the structure of the monomer.
[0068] The conjugated diene copolymer used in the modification reaction (hereinafter also referred to as "terminal modification reaction") in this process can be any copolymer with an active end, and the polymerization initiation end can be unmodified or modified. As compound (C2), there is no particular limitation as long as it is a compound that can react with the active end of the conjugated diene copolymer, but it is preferred to be a compound having one or more functional groups selected from amino, carbon-nitrogen double bond, nitrogen-containing heterocyclic group, phosphin, epoxy, thioepoxy, protected hydroxyl, protected thiol, and alkyloxysilyl groups and that can react with the polymerization active end. Specifically, as compound (C2), it is preferable to use at least one of the compounds represented by the following general formula (5) and the compounds represented by the following general formula (6).
[0069]
[0070] (In equation (5), A) 1 It has at least one atom selected from nitrogen, phosphorus, oxygen, sulfur and silicon and is related to R 5 A monovalent functional group, or a (thio)epoxy group, bonded to a nitrogen atom, phosphorus atom, oxygen atom, sulfur atom, silicon atom, or a carbon atom contained in a carbonyl group. R 3 and R 4 It is a hydrocarbon group, R 5 It is a hydrocarbon group, and r is an integer from 0 to 2. Where R... 3 and R 4 When multiple R exist, multiple R 3 and R 4 They can be the same or different.
[0071]
[0072] (In formula (6), A) 2 It has at least one atom selected from nitrogen, phosphorus, oxygen, sulfur and silicon, and does not have active hydrogen, and is related to R 9 A monovalent functional group bonded by nitrogen, phosphorus, oxygen, sulfur, or silicon atoms. R 6 and R 7 Each is an independent hydrocarbon group, R 8and R 9 Each is an independent hydrocarbon group, and m is 0 or 1. Among them, R... 7 When multiple R exist, multiple R 7 They can be the same or different.
[0073] In equations (5) and (6) above, R is used as... 3 R 4 R 6 and R 7 The hydrocarbon group is preferably a straight-chain or branched alkyl group with 1 to 20 carbon atoms, a cycloalkyl group with 3 to 20 carbon atoms, or an aryl group with 6 to 20 carbon atoms. As R 5 R 8 and R 9 The alkylene group is preferably a straight-chain or branched alkyl dimethyl alkane with 1 to 20 carbon atoms, a cycloalkylene group with 3 to 20 carbon atoms, or an arylene group with 6 to 20 carbon atoms. To improve reactivity with the active terminal, r and m are preferably 0 or 1.
[0074] A 1 When A is a monovalent functional group as described above, 1 The at least one atom selected from nitrogen, phosphorus, oxygen, sulfur, and silicon is preferably not bonded to active hydrogen but protected by a protecting group (e.g., a trisubstituted alkylsilyl group). Additionally, A 2 The at least one atom selected from nitrogen, phosphorus, oxygen, sulfur, and silicon is preferably not bonded to active hydrogen but protected by a protecting group (e.g., a trisubstituted alkylsilyl group). It should be noted that in this specification, "active hydrogen" refers to a hydrogen atom bonded to an atom other than a carbon atom, preferably a hydrogen atom with a bond energy lower than the carbon-hydrogen bond of polymethylene. A protecting group refers to the atom of A... 1 A 2 It is transformed into a functional group that is inactive at the polymerizable active end. (Thio)epoxy group refers to a group that contains both epoxy and thioepoxy groups.
[0075] A 1 Can be used The generating agent becomes Ionic groups. By giving the compound (C2) such a group (A 1 (), can impart excellent adhesion to conjugated diene copolymers. As A 1Specific examples include nitrogen-containing groups formed by replacing two hydrogen atoms of a primary amino group with two protecting groups, nitrogen-containing groups formed by replacing one hydrogen atom of a secondary amino group with one protecting group, phosphorus-containing groups formed by replacing two hydrogen atoms of a tertiary amino group, imino group, pyridyl group, or primary phosphinyl group with two protecting groups, phosphorus-containing groups formed by replacing one hydrogen atom of a secondary phosphinyl group with one protecting group, groups where the hydrogen atoms of a tertiary phosphinyl group, epoxy group, or hydroxyl group are protected by protecting groups, sulfur-containing groups formed by replacing the hydrogen atoms of a thioepoxy group or thiol group with protecting groups, and alkyloxycarbonyl groups, etc. Among these, groups having nitrogen atoms are preferred due to their good affinity for solid electrolytes and active substances, and more preferably nitrogen-containing groups formed by replacing two hydrogen atoms of a tertiary amino group or a primary amino group with two protecting groups.
[0076] Preferred specific examples of compound (C2) include dibutylsilicon dichloride, methylsilicon trichloride, dimethylsilicon dichloride, silicon tetrachloride, triethoxymethylsilane, triphenoxymethylsilane, trimethoxysilane, methyltriethoxysilane, compounds represented by the above general formula (5), and compounds represented by the above general formula (6). Examples of compounds represented by the above general formula (5) include N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N-trimethylsilyl-N-methylaminopropylmethyldiethoxysilane, [3-(N,N-dimethylamino)propyl]trimethoxysilane, N,N',N'-tri(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-(4-trimethylsilyl-1-piperazinyl)propylmethyldimethoxysilane, 3-epoxypropoxypropylmethyldimethoxysilane, and 3-epoxypropoxypropyltriethoxysilane. In addition, examples of compounds represented by the above general formula (6) include 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1,2-azasilcyclopentane, 2,2-dimethoxy-1-phenyl-1,2-azasilcyclopentane, 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silcyclopentane, and 2,2-dimethoxy-8-(4-methylpiperazinyl)methyl-1,6-dioxa-2-silcyclooctane. Compound (C2) can be used alone or in combination of two or more.
[0077] In addition to compound (C2), germane compounds, tin compounds, etc., may also be appropriately used in the modification process. By using these compounds, germanium atoms and tin atoms can be introduced into the conjugated diene copolymer (A). It should be noted that in this specification, the group of compounds (R), (C2), germane compounds, and tin compounds is also referred to as "modifiers".
[0078] Examples of germane compounds include, for instance, monoalkoxygermane compounds, dialkoxygermane compounds, trimekoxygermane compounds, and tetraalkoxygermane compounds; halogenated triorganogermane compounds, dihalogenated diorganogermane compounds, trihalogenated organogermane compounds, and tetrahalogenated germane compounds. Furthermore, examples of germane compounds include compounds similar to those exemplified as silane compounds, but with germanium atoms replacing silicon atoms.
[0079] Examples of the aforementioned tin alkane compounds include, for example, monoalkoxytin alkane compounds, dialkoxytin alkane compounds, trialkoxytin alkane compounds, tetraalkoxytin alkane compounds, and other alkoxytin alkane compounds; halogenated triorganotin alkane compounds, dihalogenated diorganotin alkane compounds, trihalogenated organotin alkane compounds, and tetrahalogenated tin alkane compounds. Furthermore, examples of the aforementioned tin alkane compounds include compounds that, like the compounds exemplified as silane compounds, have tin atoms replacing silicon atoms.
[0080] Specific examples of these tin alkyl compounds include tin tetrachloride, tin tetrabromide, trichlorobutyltin, trichloromethyltin, trichlorooctyltin, dibromodimethyltin, dichlorodimethyltin, dichlorodibutyltin, dichlorodioctyltin, 1,2-bis(trichloromethyltinyl)ethane, 1,2-bis(methyldichloromethyltinyl)ethane, 1,4-bis(trichloromethyltinyl)butane, 1,4-bis(methyldichloromethyltinyl)butane, ethyltin tristearate, butyltin trioctanoate, butyltin tristearate, butyltin trilaurate, dibutyltin dioctanoate, dibutyltin distearate, and dibutyltin dilaurate. Tin tetrachloride (SnCl4) is particularly preferred.
[0081] The aforementioned end-modification reaction can be carried out, for example, as a solution reaction. This solution reaction can be carried out using a solution containing unreacted monomers after the polymerization reaction in the aforementioned polymerization step, or it can be carried out after separating and dissolving the conjugated diene copolymer contained in the solution in a suitable solvent such as cyclohexane. Furthermore, the end-modification reaction can be carried out using either a batch or continuous process. In this case, there are no particular limitations on the method of adding the compound (C2), germane compound, or tin alkane compound; examples include simultaneous addition, batch addition, and continuous addition.
[0082] The amount of the compound (C2), germane compound, or tin alkane compound used in the end-modification reaction can be appropriately set according to the type of compound used in the reaction. It is preferably 0.1 molar equivalents or more, more preferably 0.3 molar equivalents or more, relative to the metal atoms participating in the polymerization reaction of the polymerization initiator. By using an amount of 0.1 molar equivalents or more, the modification reaction can be fully carried out, and the dispersion stability of the slurry can be appropriately improved.
[0083] The temperature of the end-modification reaction is usually the same as that of the polymerization reaction described above, preferably -20 to 150°C, more preferably 0 to 120°C, and particularly preferably 20 to 100°C. If the temperature of the modification reaction is low, there is a tendency for the viscosity of the modified conjugated diene copolymer to increase. On the other hand, if the temperature of the modification reaction is high, the polymeric active ends become more easily deactivated. The reaction time of the modification reaction is preferably 1 minute to 5 hours, more preferably 2 minutes to 1 hour.
[0084] As described above, the conjugated diene copolymer (A) preferably has units based on a modifier comprising at least one atom selected from nitrogen, oxygen, silicon, germanium, and tin. By incorporating units based on such a modifier into the conjugated diene copolymer (A), the dispersion stability of the slurry is improved, thus enhancing the formability of the pressurized form of the all-solid-state secondary battery. Consequently, an all-solid-state secondary battery with excellent lithium-ion conductivity and good cycle life characteristics is obtained.
[0085] < Agent addition process >
[0086] When the conjugated diene copolymer (A) has units based on a nitrogen-containing modifier, an additive can be added after the above-mentioned modification process. The process of generating the agent. This is achieved by adding... The generating agent can impart shape stability to the conjugated diene copolymer (A). Additionally, if the amount of... The amount of generating agent added tends to increase the storage modulus (G') of the conjugated diene copolymer (A).
[0087] As Examples of generating agents include silicon halide compounds, tin halide compounds, aluminum halide compounds, titanium halide compounds, zirconium halide compounds, germanium halide compounds, gallium halide compounds, zinc halide compounds, and other halide metals; hydrofluoric acid, hydrochloric acid, hydrobromic acid, iodic acid, sulfuric acid, nitric acid, carbonic acid, phosphoric acid, and other inorganic acids; potassium fluoride, tetramethylammonium fluoride, tetra-n-butylammonium fluoride, and other inorganic acid salts; and carboxylic acids, sulfonic acids, sulfate esters, phosphate esters, carbonates, nitrate esters, and other organic acids.
[0088] As Examples of generating compounds include metal halides such as silicon tetrachloride, tin tetrachloride, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, methyldichlorosilane, diethylaluminum chloride, sesquiethylaluminum chloride, ethylaluminum dichloride, titanium tetrachloride, dicerocene dichloride, zirconium tetrachloride, dicerocene dichloride, germanium tetrachloride, gallium trichloride, and zinc chloride. Additionally, other... Examples of compounds that can generate these agents include diethyl sulfate, dimethyl sulfate, magnesium lauryl ether sulfate, magnesium lauryl sulfate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, 2-ethylhexyl phosphate, triphenyl phosphate, tricresyl phosphate, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, nitrocellulose, nitroglycerin, nitroethylene glycol, formic acid, acetic acid, oxalic acid, maleic acid, citric acid, malic acid, fumaric acid, malonic acid, acrylic acid, crotonic acid, succinic acid, glutaric acid, itaconic acid, tartaric acid, sebacic acid, terephthalic acid, isophthalic acid, β-mercaptopropionic acid, benzenesulfonic acid, p-toluenesulfonic acid, hydrofluoric acid, hydrochloric acid, hydrobromic acid, iodic acid, sulfuric acid, nitric acid, carbonic acid, phosphoric acid, potassium fluoride, tetramethylammonium fluoride, tetra-n-butylammonium fluoride, etc. These can be derived from units based on modifiers containing nitrogen atoms. From a cultural perspective, these All generating agents have the same function and can be used in this invention even if they are not described in the examples described later.
[0089] The modified conjugated diene copolymer obtained in the modification process and The mixing of the generating agents can be carried out, for example, in solution form. There are no particular restrictions on the form of mixing; it can be carried out using batch mixers or continuously using multi-stage continuous mixers, online agitators, or other similar devices.
[0090] can be The amount of acidic component generated by the generating agent is preferably 1.0 molar equivalent or more, more preferably 1.5 molar equivalent or more, relative to the active site of the conjugated diene copolymer obtained by anionic polymerization. If it is less than 1.0 molar equivalent, then sometimes... Incomplete chemical processing results in poor shape retention of the rubber.
[0091] Here, it can be obtained from The amount of acid produced by the generating agent is expressed as follows.
[0092] · When the generating agent has hydrogen atoms with a pKa of 7 or less as measured in water at 25°C: The amount of hydrogen atoms present in the water of the generating agent with a pKa of 7 or less, as measured at 25°C.
[0093] · When the generating agent does not possess hydrogen atoms with a pKa of less than 7 as measured in water at 25°C and generates hydrogen ions upon contact with water: The amount of hydrogen ions produced when 100 mol of water is added to the generating agent and the reaction is carried out at 25°C for a sufficient time.
[0094] · When the generating agent does not contain hydrogen atoms with a pKa of less than 7 as measured in water at 25°C and does not release hydrogen ions upon contact with water: The amount of the generating agent.
[0095] There are no particular restrictions on the method of adding the generating agent; methods such as adding it all at once, adding it in batches, or adding it continuously can be cited, with adding it all at once being preferred. Furthermore, The generating agent may also be added in the form of a solution of hydrocarbon solvents such as aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons, which are used as organic solvents in the polymerization process described above, as well as randomizing agents.
[0096] The modified conjugated diene copolymer obtained in the modification process and The mixing temperature of the generating agent can be directly used as the polymerization temperature of the polymerization process described above. Specifically, it is preferably 0 to 120°C, more preferably 20 to 100°C. If the temperature is too low, the viscosity of the polymer tends to increase; if the temperature is too high, the active ends of the polymerization are prone to deterioration. Therefore, temperatures outside the above-mentioned ranges are not preferred. In addition, the mixing time is preferably 1 minute to 5 hours, more preferably 2 minutes to 1 hour.
[0097] <Anti-aging agent addition process>
[0098] After the above modification process or with the addition A step of adding an anti-aging agent can be set after the formation agent step. By adding an anti-aging agent, it is possible to prevent gelation and deterioration of the conjugated diene copolymer (A) due to heat, light and oxidation during the stripping-based desolventizing process, the hot roller drying process, and the subsequent long-term storage in packaged form.
[0099] Examples of anti-aging agents include phenolic anti-aging agents, amine-based anti-aging agents, quinone-based anti-aging agents, phosphorus-based anti-aging agents, sulfur-based anti-aging agents, and phenothiazine-based anti-aging agents. Among these, phenolic and amine-based anti-aging agents are preferred. These anti-aging agents can be used alone or in combination of two or more.
[0100] Examples of phenolic anti-aging agents include, for example, p-methoxyphenol, 2,6-di-tert-butyl-p-cresol, phenol, hydroquinone, p-cresol, butylated hydroxyanisole, propyl gallate, chlorogenic acid, catechin, caffeic acid, genistein, luteolin, tocopherol, catechol, resorcinol, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, pyrogallol, 4,4'-butylidenebis(6-tert-butyl-m-cresol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), and 2,2'-methylenebis(6-tert-butyl-4-ethyl-2 ... 4,4'-Thiobis(6-tert-butyl-m-cresol), 2,5-di-tert-pentylhydroquinone, stylated phenol, 2,5-di-tert-butylhydroquinone, 2-methyl-4,6-bis[(n-octylthio)methyl]phenol, 2,4-bis(dodecylthiomethyl)-6-methylphenol, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate.
[0101] Examples of amine-based anti-aging agents include 1-naphthylamine, 2-naphthylamine, phenylenediamine, 4,4'-diaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, N-isopropyl-N'-phenylphenyl-1,4-diamine, N-(1,3-dimethylbutyl)-N'-phenyl-1,4-phenylenediamine, 2,2,4-trimethyl-1,2-dihydroquinoline polymer, and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, among other aromatic amines. Additionally, photostabilizers (HALS), hindered amine compounds, and nitryl radicals (2,2,6,6-tetramethylpiperidine-1-oxy(TEMPO)) can also be used as amine-based anti-aging agents.
[0102] Phosphite compounds can be cited as phosphorus-based anti-aging agents. Thiol compounds and sulfur compounds such as pentaerythritol tetra(3-lauryl thiopropionate) can be used as sulfur-based anti-aging agents.
[0103] The aforementioned anti-aging agent can be added in any of the following states: solid, molten, or in solution dissolved in a solvent. The conjugated diene copolymer (A) can be in either a solid or solution state when the anti-aging agent is added; however, from the viewpoint of the dispersibility of the anti-aging agent, a solution state is preferred.
[0104] When the conjugated diene copolymer (A) contains an anti-aging agent, the lower limit of the content of the anti-aging agent relative to 100 parts by weight of the conjugated diene copolymer (A) is preferably 0.05 parts by weight, more preferably 0.1 parts by weight, and particularly preferably 0.2 parts by weight. Furthermore, the upper limit of the content of the anti-aging agent is preferably 2 parts by weight, more preferably 1.5 parts by weight, and particularly preferably 1.2 parts by weight.
[0105] <Hydrogenation Process>
[0106] The conjugated diene copolymer (A) can also be a polymer obtained by hydrogenating the modified or unmodified conjugated diene copolymer obtained above. Any method and condition can be used for the hydrogenation reaction, as long as the desired hydrogenation rate of the conjugated diene copolymer can be obtained. Examples of these hydrogenation methods include methods using catalysts with titanium-based organometallic compounds as the main component; methods using catalysts composed of organometallic compounds such as iron, nickel, and cobalt, and alkylaluminum; methods using organic complexes of organometallic compounds such as ruthenium and rhodium; and methods using catalysts with metals such as palladium, platinum, ruthenium, cobalt, and nickel supported on supports such as carbon, silica, and alumina. Among various methods, the hydrogenation method using a single organometallic compound of titanium or a homogeneous catalyst composed of an organometallic compound of titanium and organometallic compounds of lithium, magnesium, and aluminum (catalysts described in Japanese Patent Publication No. 63-4841, Japanese Patent Publication No. 1-37970, Japanese Patent Application Publication No. 2000-037632, etc.) under mild conditions of low pressure and low temperature is industrially preferred. Moreover, it also has high selectivity for hydrogenation of the double bond of butadiene, which is suitable for the purpose of this invention.
[0107] The hydrogenation reaction of the modified conjugated diene copolymer is carried out in a solvent that is inactive to the catalyst and soluble in the conjugated diene copolymer. Preferred solvents include aliphatic hydrocarbons such as n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane and cycloheptane; aromatic hydrocarbons such as benzene and toluene; and ethers such as diethyl ether and tetrahydrofuran, either alone or in mixtures thereof.
[0108] Hydrogenation reactions are generally carried out by maintaining a conjugated diene copolymer at a specified temperature in a hydrogen or inactive atmosphere, adding a hydrogenation catalyst with or without stirring, and then introducing hydrogen gas and pressurizing it to a specified pressure. An inactive atmosphere refers to an atmosphere that does not react with the participants in the hydrogenation reaction; examples include helium, neon, and argon. Air and oxygen will oxidize the catalyst, leading to catalyst deactivation, and are therefore undesirable. Furthermore, nitrogen acts as a catalyst poison during hydrogenation, reducing hydrogenation activity, and is therefore also undesirable. In particular, a hydrogen-only atmosphere is most suitable for the hydrogenation reactor.
[0109] The hydrogenation process for obtaining the hydrogenated conjugated diene copolymer can be carried out using batch, continuous, or combinations thereof. Furthermore, when using a diaryldipentadiene compound as the hydrogenation catalyst, it can be added directly to the reaction solution alone or as a solution of an inactive organic solvent. When using the catalyst in solution form, the inactive organic solvent used can be any solvent that does not react with the hydrogenation participants. Preferably, it is the same solvent used in the hydrogenation reaction. Additionally, the amount of catalyst added is 0.02–20 mmol relative to 100 g of the conjugated diene copolymer before hydrogenation.
[0110] A preferred method for obtaining the conjugated diene copolymer (A) is to perform solution polymerization of a monomer containing butadiene in the presence of an alkali metal compound, and then directly use the resulting polymer solution for a modification step, which is industrially useful. Alternatively, a hydrogenation step may be included after the modification step. In this case, the conjugated diene copolymer (A) is obtained by removing the solvent from the solution obtained above and separating the conjugated diene copolymer (A). Separation of the conjugated diene copolymer (A) can be carried out using known desolventizing methods such as stripping and drying operations such as heat treatment.
[0111] In terms of improving the dispersion stability of the slurry and the adhesion of the electrodes, the conjugated diene copolymer (A) preferably has one or more functional groups selected from amino, nitrogen-containing heterocyclic, phosphin, hydroxyl, thiol, and hydroxyloxysilyl groups, and more preferably has one or more functional groups selected from amino, nitrogen-containing heterocyclic, and hydroxyloxysilyl groups. It is particularly preferred to introduce these functional groups into the ends of the conjugated diene copolymer (A).
[0112] 1.2. Properties of the conjugated diene copolymer (A)
[0113] <Storage elastic modulus (G') and loss tangent (tanδ)>
[0114] The storage modulus (G') of the conjugated diene copolymer (A) is 4.0 × 10⁻⁶. 4 Pa ~ 2.0 × 10 5 Pa. The lower limit of the storage modulus (G') of the conjugated diene copolymer (A) is preferably 4.5 × 10⁻⁶. 4 Pa, more preferably 5.0 × 10 Pa. 4 Pa, preferably 5.5 × 10 Pa. 4 Pa. The upper limit of the storage modulus (G') of the conjugated diene copolymer (A) is preferably 1.9 × 10⁻⁶. 5 Pa, more preferably 1.8 × 10 Pa 5 Pa, preferably 1.7 × 10 Pa. 5Pa. If the storage modulus (G') of the conjugated diene copolymer (A) is above or above the aforementioned lower limit, the electrode strength is improved, and a good electrode can be obtained. Furthermore, by ensuring that the storage modulus (G') of the conjugated diene copolymer (A) is within the aforementioned range, the obtained electrode possesses appropriate flexibility, thus reducing the likelihood of powdering or cracking after coating or pressing. Additionally, an electrode with good adhesion and excellent energy storage device characteristics is obtained.
[0115] The loss tangent (tanδ) of the conjugated diene copolymer (A) is 0.10 to 0.80. The lower limit of the loss tangent (tanδ) of the conjugated diene copolymer (A) is preferably 0.12, more preferably 0.14, and particularly preferably 0.16. The upper limit of the loss tangent (tanδ) of the conjugated diene copolymer (A) is preferably 0.78, more preferably 0.76, and particularly preferably 0.74. If the loss tangent (tanδ) of the conjugated diene copolymer (A) is above the above lower limit, the adhesion of the obtained electrode is improved, and powder shedding and cracking after coating and pressing are less likely to occur. Furthermore, by keeping the loss tangent (tanδ) of the conjugated diene copolymer (A) within the above range, an electrode that can suppress the increase in electrode resistance and also has good energy storage device characteristics can be obtained.
[0116] The storage modulus and loss tangent of the conjugated diene copolymer (A) can be determined as follows. First, the conjugated diene copolymer (A) is dissolved in a desired organic solvent, and the solution is dried to prepare a uniform film with a thickness of 1.0 ± 0.3 mm. The film is further dried, and strips of 10 mm × 10 mm are cut out as samples for measurement. Next, using a dynamic viscoelasticity measuring device (e.g., Anton Paar, model "MCR 301"), the samples are fixed with parallel plates, and dynamic viscoelasticity is measured under shear mode, a measurement temperature of 25 °C, a frequency of 0.1 Hz, and a strain of 1%. The values of the storage modulus and loss tangent can be obtained.
[0117] It should be noted that the storage modulus (G') and loss tangent (tanδ) of the conjugated diene copolymer (A) can be adjusted, for example, by changing the composition, microstructure, molecular weight, and terminal functional groups (polymerization initiation end and polymerization termination end) of the conjugated diene copolymer (A). Specifically, the storage modulus (G') of the conjugated diene copolymer (A) decreases when the bonded styrene content is reduced, and increases when the polymerization termination end is functionalized. Furthermore, the loss tangent (tanδ) decreases when the polymerization termination end is functionalized.
[0118] <Bonded styrene content>
[0119] The lower limit of the bonded styrene content in the conjugated diene copolymer (A) is preferably 5%, more preferably 8%, and particularly preferably 10%. The upper limit of the bonded styrene content in the conjugated diene copolymer (A) is preferably 45%, more preferably 30%, and particularly preferably 27%. If the bonded styrene content of the conjugated diene copolymer (A) is within the above range, it is possible to achieve both good adhesion and flexibility of the electrode. It should be noted that the bonded styrene content can be adjusted by... 1 The determination was made using H-NMR.
[0120] <Weight-average molecular weight>
[0121] The weight-average molecular weight (Mw) of the conjugated diene copolymer (A) is preferably 1.0 × 10⁻⁶. 5 ~2.0×10 6 More preferably 1.0×10 5 ~1.5×10 6 The preferred value is 1.5×10. 5 ~1.0×10 6 If the weight-average molecular weight (Mw) is above the lower limit mentioned above, there is a tendency to improve the adhesion of the electrode. If the weight-average molecular weight (Mw) is below the upper limit mentioned above, there is a tendency to maintain the flexibility of the electrode. It should be noted that in this specification, "weight-average molecular weight (Mw)" refers to the weight-average molecular weight of polystyrene determined by gel permeation chromatography (GPC).
[0122] <Hydrogenation rate>
[0123] As described above, the conjugated diene copolymer (A) can also be a hydrogenated polymer. In this case, the conjugated diene copolymer (A) has at least any one of the structural units represented by formula (1), formula (2), formula (3), and formula (4). When the composition ratio (molar ratio) in the polymer is set to p, q, r, and s, respectively, the value α represented by the following mathematical formula (i) corresponds to the hydrogenation rate of the conjugated diene copolymer. For example, when α in the following mathematical formula (i) is 0.7, the hydrogenation rate of the conjugated diene copolymer is 70%.
[0124] α=(p+(0.5×r)) / (p+q+(0.5×r)+s)···(i)
[0125]
[0126] α can take any value, but by setting it to less than 0.7, high lithium-ion conductivity and good cycle life characteristics can be achieved while maintaining excellent slurry dispersion stability and electrode flexibility. For this reason, α is preferably less than 0.7, more preferably less than 0.6, and particularly preferably less than 0.5. The hydrogenation rate in the conjugated diene copolymer can be adjusted according to the hydrogenation reaction time or the amount of hydrogen supplied, etc. This hydrogenation rate can be... 1 The measurements were performed using H-NMR.
[0127] 2. Binder composition for all-solid-state secondary batteries
[0128] One embodiment of the present invention provides an all-solid-state secondary battery binder composition comprising the aforementioned all-solid-state secondary battery binder and a liquid medium (B). Hereinafter, each component contained in the all-solid-state secondary battery binder composition of this embodiment will be described in detail. It should be noted that the all-solid-state secondary battery binder has already been described above, therefore a detailed description is omitted.
[0129] 2.1. Liquid medium (B)
[0130] As a liquid medium (B), there are no particular limitations, and aliphatic hydrocarbons such as hexane, heptane, octane, decane, and dodecane; alicyclic hydrocarbons such as cyclohexane, cycloheptane, cyclooctane, and cyclodecane; aromatic hydrocarbons such as toluene, xylene, mesitylene, naphthalene, and tetrahydronaphthalene; ketones such as 3-pentanone, 4-heptanone, methyl hexyl ketone, and diisobutyl ketone; esters such as butyl acetate, butyl butyrate, methyl butyrate, butyl valerate, butyl hexanoate, pentyl butyrate, pentyl valerate, pentyl hexanoate, hexyl valerate, and hexyl hexanoate; and ethers such as dibutyl ether, tetrahydrofuran, and anisole can be used. These solvents can be used alone or in combination of two or more.
[0131] The content of the liquid medium (B) relative to 100 parts by weight of the conjugated diene copolymer (A) is preferably 100 to 10,000 parts by weight, more preferably 150 to 5,000 parts by weight, even more preferably 200 to 4,000 parts by weight, and particularly preferably 300 to 3,000 parts by weight. By keeping the content of the liquid medium (B) within the above range, the workability of the all-solid-state secondary battery binder composition and the all-solid-state secondary battery slurry obtained from the composition can be improved.
[0132] <Solubility>
[0133] In the all-solid-state secondary battery binder composition of this embodiment, the conjugated diene copolymer (A) is preferably dissolved in the liquid medium (B). "The conjugated diene copolymer (A) is dissolved in the liquid medium (B)" means that the solubility of the conjugated diene copolymer (A) in the liquid medium (B) is 1 g or more relative to 100 g of the liquid medium (B). By ensuring that the conjugated diene copolymer (A) is dissolved in the liquid medium (B), it is easy to coat the surface of the active material with the flexible and well-adhesive conjugated diene copolymer (A). Therefore, it is possible to effectively suppress shedding caused by the stretching and contraction of the active material during charging and discharging, and easily obtain an all-solid-state secondary battery exhibiting excellent charge-discharge durability characteristics. Furthermore, the slurry has good stability and good coating properties to the current collector, which is also preferable.
[0134] 2.2. Other additives
[0135] The all-solid-state secondary battery binder composition of this embodiment may contain additives such as anti-aging agents and thickeners as needed.
[0136] Anti-aging agents
[0137] As anti-aging agents, various anti-aging agents described in the "Anti-aging Agent Addition Step" section of "1.1. Method for Manufacturing Conjugated Diene Copolymer (A)" above can be cited.
[0138] When the all-solid secondary battery binder composition of this embodiment contains an anti-aging agent, the proportion of the anti-aging agent relative to 100 parts by weight of all solid components of the all-solid secondary battery binder composition is preferably 0.05 to 2 parts by weight, more preferably 0.1 to 1 parts by weight, and particularly preferably 0.2 to 0.8 parts by weight.
[0139] <Thickener>
[0140] By including thickeners, it is sometimes possible to further improve the coatability and charge / discharge characteristics of the resulting all-solid-state secondary battery.
[0141] Examples of thickeners include, for example, cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, ethyl cellulose, and hydroxypropyl cellulose; poly(meth)acrylic acid; the above-mentioned cellulose compounds or ammonium or alkali metal salts of the above-mentioned poly(meth)acrylic acid; modified polyvinyl alcohol, polyethylene oxide; polyvinylpyrrolidone, polycarboxylic acid, oxidized starch, phosphate starch, casein, various modified starches, chitin, chitosan derivatives, etc. Among these, cellulose-based polymers are preferred.
[0142] When the all-solid secondary battery binder composition of this embodiment contains a thickener, the proportion of the thickener relative to 100 parts by weight of all solid components of the all-solid secondary battery binder composition is preferably 5 parts by weight or less, and more preferably 0.1 to 3 parts by weight.
[0143] 2.3. Preparation method of binder composition for all-solid-state secondary batteries
[0144] The all-solid-state binder composition for secondary batteries of this embodiment can be prepared by the following steps: adding a liquid medium (B) to a conjugated diene copolymer (A), further adding other additives as needed, and stirring appropriately to dissolve or disperse the conjugated diene copolymer (A) in the liquid medium (B).
[0145] The binder composition for all-solid-state secondary batteries of this embodiment can form a binder that has high adhesion not only to the current collector of the electrode but also to the solid electrolyte material. It can reduce the amount used and improve the conductivity of the solid electrolyte layer, and is therefore preferred for use in all-solid-state batteries.
[0146] The method for preparing the all-solid-state secondary battery binder composition according to this embodiment may include a step of removing particulate metal components from the binder composition (hereinafter also referred to as the "particulate metal removal step"). In the particulate metal removal step, "particulate metal components" refers to metal components that exist in the binder composition in a particulate form, excluding metal components that exist in a dissolved state as metal ions.
[0147] The method for removing particulate metal components from the binder composition for all-solid-state secondary batteries in the particulate metal removal process is not particularly limited. For example, methods such as removal by filtration using a filter, removal by a vibrating screen, removal by centrifugation, and removal by magnetic force can be cited. Among these, since the object to be removed is a metal component, the method of removal by magnetic force is preferred.
[0148] As for the method of removing metal components using magnetic force, there is no particular limitation as long as the method can remove the metal components. However, if productivity and removal efficiency are taken into consideration, it is preferable to remove the polymer solution by equipping a magnetic filter in the production line of the all-solid secondary battery binder composition.
[0149] The process of removing particulate metal components from a polymer solution using a magnetic filter is preferably performed by passing the solution through a magnetic filter that generates a magnetic flux density of 100 Gauss or higher. If the magnetic flux density is low, the removal efficiency of the metal components decreases; therefore, a magnetic flux density of 1000 Gauss or higher is preferred. If the removal of weakly magnetic stainless steel is taken into consideration, a magnetic flux density of 2000 Gauss or higher is even more preferred, and a magnetic flux density of 5000 Gauss or higher is most preferred.
[0150] When configuring a magnetic filter in a production line, it is preferable to include a process upstream of the magnetic filter where a cartridge filter or similar filter is used to remove large foreign objects or metal particles. This is because large metal particles may pass through the magnetic filter due to the flow rate during filtration.
[0151] Furthermore, while magnetic filters are effective even with only one pass, a recirculating filter is preferable. This is because a recirculating filter increases the efficiency of metal particle removal.
[0152] When a magnetic filter is installed in a production line for the binder composition for all-solid-state secondary batteries, there are no particular restrictions on the location of the magnetic filter. However, it is preferable to install it before the filter, especially if there is a filter-based filtration process before filling the container with the binder composition for all-solid-state secondary batteries. This is because the magnetic filter prevents the contamination of metal components into the product.
[0153] Specific examples of particulate metal components include metals such as Fe, Ni, and Cr, or their metal compounds. The all-solid-state binder composition for secondary batteries of this embodiment sometimes contains residual particulate metal components. It is preferable to remove these particulate metal components using a particulate metal removal process to reduce the content of particulate metal components with a particle size of 20 μm or more to 10 ppm or less. To determine the content of particulate metal components with a particle size of 20 μm or more, the obtained all-solid-state binder composition for secondary batteries can be further filtered through a sieve with a mesh size equivalent to 20 μm. Elemental analysis of the metal particles on the sieve is performed using an X-ray microanalyzer (EPMA), and the solution after dissolving the metal in an acid capable of dissolving it is measured using ICP (Inductively Coupled Plasma).
[0154] 3. Slurry for all-solid-state secondary batteries
[0155] One embodiment of the present invention provides a slurry for an all-solid-state secondary battery comprising the aforementioned binder composition for all-solid-state secondary batteries and a solid electrolyte. This all-solid-state slurry for a secondary battery can also be used as a material for forming either a positive electrode active material layer or a negative electrode active material layer, and further, as a material for forming a solid electrolyte layer.
[0156] The all-solid-state slurry for forming the positive electrode active material layer of a secondary battery contains the aforementioned all-solid-state secondary battery binder composition, solid electrolyte, and positive electrode active material (hereinafter also simply referred to as "positive electrode active material"). Furthermore, the all-solid-state secondary battery slurry for forming the negative electrode active material layer contains the aforementioned all-solid-state secondary battery binder composition, solid electrolyte, and negative electrode active material (hereinafter also simply referred to as "negative electrode active material"). Moreover, the all-solid-state secondary battery slurry for forming the solid electrolyte layer contains the aforementioned all-solid-state secondary battery binder composition and solid electrolyte. Hereinafter, the components that may be included in the all-solid-state secondary battery slurry of this embodiment will be described.
[0157] 3.1. Active substances
[0158] <Positive Electrode Active Material>
[0159] As positive electrode active materials, for example, MnO2, MoO3, V2O5, and V6O can be used. 13 Fe2O3, Fe3O4, Li (1-x) CoO2, Li (1-x) NiO2, Li x Co y Sn z O2, Li (1-x) Co (1-y) Ni y O2, Li (1+x) Ni 1 / 3 Co 1 / 3 Mn 1 / 3 Inorganic compounds such as O2, TiS2, TiS3, MoS3, FeS2, CuF2, and NiF2; carbon materials such as fluorinated carbon, graphite, vapor-grown carbon fibers and / or their pulverized forms, PAN-based carbon fibers and / or their pulverized forms, and pitch-based carbon fibers and / or their pulverized forms; and conductive polymers such as polyacetylene and poly(p-phenylene). These positive electrode active materials can be used individually or in combination of two or more.
[0160] The average particle size of the positive electrode active material is not particularly limited, but to increase the contact area at the solid-solid interface, a particle size of 0.1 μm to 50 μm is preferred. To achieve the specified average particle size, pulverizers such as mortars, ball mills, sand mills, vibratory ball mills, planetary ball mills, and cyclone mills, as well as classifiers such as sieves and air classifiers, can be used. During pulverization, wet pulverization with solvents such as water or methanol can be performed as needed. Classification can be done using either dry or wet methods. Furthermore, the positive electrode active material obtained by calcination can be used after washing with water, acidic aqueous solutions, alkaline aqueous solutions, or organic solvents.
[0161] It should be noted that the average particle size of the active material refers to the volume average particle size measured using a particle size distribution measuring device based on laser diffraction. Examples of such laser diffraction particle size distribution measuring devices include the HORIBALA-300 series and the HORIBALA-920 series (both manufactured by Horiba Manufacturing Co., Ltd.).
[0162] In the all-solid-state slurry for forming the positive electrode active material layer, the proportion of positive electrode active material is preferably 20 to 90 parts by mass when the total solid components are set to 100 parts by mass, and more preferably 40 to 80 parts by mass.
[0163] <Negative Electrode Active Material>
[0164] As a negative electrode active material, there are no particular limitations as long as it can reversibly adsorb and release lithium ions. Examples include carbonaceous materials, metal oxides such as tin oxide and silicon oxide, elemental lithium, lithium alloys such as lithium-aluminum alloys, and metals that can form alloys with lithium such as Sn, Si, or In. Among these, carbonaceous materials are preferred from a reliability perspective, while silicon-containing materials are preferred from the perspective of increasing battery capacity.
[0165] As a carbonaceous material, there are no particular limitations as long as it is substantially composed of carbon. Examples include petroleum asphalt, natural graphite, vapor-grown graphite, and other artificial graphite, as well as carbonaceous materials obtained by calcining various synthetic resins such as PAN-based resins and furfuryl alcohol resins. Furthermore, examples include various types of carbon fibers such as PAN-based carbon fibers, cellulose-based carbon fibers, pitch-based carbon fibers, vapor-grown carbon fibers, dehydrated PVA-based carbon fibers, lignin carbon fibers, glassy carbon fibers, and activated carbon fibers, as well as mesophase microspheres, graphite whiskers, and planar graphite.
[0166] Compared to commonly used graphite and acetylene black, silicon-containing materials can retain more lithium ions. That is, due to the increased lithium ion retention per unit weight, the battery capacity can be increased. As a result, it has the advantage of longer battery operating time, and is expected to be used in future automotive batteries, etc. On the other hand, it is known that silicon-containing materials experience significant volume changes with lithium ion retention and release; the volume expansion based on lithium ion retention in graphite and acetylene black is about 1.2 to 1.5 times, while in silicon-containing negative electrode active materials it is sometimes about 3 times. Repeated expansion and contraction (charge and discharge) leads to insufficient durability of the negative electrode active material layer, sometimes causing insufficient contact or a shorter cycle life (battery life). The negative electrode active material layer formed using the all-solid-state secondary battery slurry of this embodiment exhibits high durability (strength) because the binder component follows even with repeated expansion and contraction, thus achieving excellent cycle life characteristics.
[0167] The average particle size of the negative electrode active material is not particularly limited, but it is preferably 0.1 μm to 60 μm in order to increase the contact area at the solid-solid interface. To ensure that the negative electrode active material has the specified average particle size, the pulverizer or classifier exemplified above can be used.
[0168] In the all-solid-state slurry for forming the negative electrode active material layer, the proportion of negative electrode active material is preferably 20 to 90 parts by mass when the total solid components are set to 100 parts by mass, and more preferably 40 to 80 parts by mass.
[0169] 3.2. Solid electrolytes
[0170] The slurry for an all-solid-state secondary battery according to this embodiment contains a solid electrolyte. As the solid electrolyte, a solid electrolyte commonly used in all-solid-state secondary batteries can be appropriately selected and used, preferably a sulfide-based solid electrolyte or an oxide-based solid electrolyte.
[0171] The lower limit of the average particle size of the solid electrolyte is preferably 0.01 μm, more preferably 0.1 μm. The upper limit of the average particle size of the solid electrolyte is preferably 100 μm, more preferably 50 μm.
[0172] In the all-solid-state secondary battery slurry of this embodiment, to achieve both battery performance and the reduction and maintenance of interfacial resistance, when the total solid components are set to 100 parts by mass, the lower limit of the solid electrolyte content is preferably 50 parts by mass, more preferably 70 parts by mass, and particularly preferably 90 parts by mass. For the upper limit of the solid electrolyte content, for the same effect, when the total solid components are set to 100 parts by mass, the upper limit is preferably 99.9 parts by mass, more preferably 99.5 parts by mass, and particularly preferably 99.0 parts by mass. When used together with the aforementioned positive electrode active material or the aforementioned negative electrode active material, their total concentration is preferably within the above-mentioned concentration range.
[0173] <Sulfide-based solid electrolytes>
[0174] Sulfide-based solid electrolytes preferably contain sulfur atoms (S) and metal elements of Group IA or IIA of the periodic table, and possess ionic conductivity and electronic insulation. Examples of such sulfide-based solid electrolytes include those with the composition represented by the following general formula (7).
[0175] Li a M b P c S d ·····(7)
[0176] (In equation (7), M represents an element selected from B, Zn, Si, Cu, Ga, and Ge. a to d represent the composition ratio of each element, satisfying a:b:c:d = 1 to 12:0 to 1:1:2 to 9.)
[0177] In the above general formula (7), the composition ratio of Li, M, P and S is preferably b = 0. More preferably, b = 0, and a:c:d = 1 to 9:1:3 to 7. Even more preferably, b = 0, and a:c:d = 1.5 to 4:1:3.25 to 4.5. As will be described later, the composition ratio of each element can be controlled by adjusting the amount of raw material compounds used in the manufacture of sulfide-based solid electrolytes.
[0178] Sulfide-based solid electrolytes can be amorphous (glass), crystalline (glass ceramic), or only partially crystallized.
[0179] In Li-P-S glass and Li-P-S glass-ceramics, the ratio of Li₂S to P₂S₅, expressed as a molar ratio of Li₂S:P₂S₅, is preferably 65:35 to 85:15, more preferably 68:32 to 80:20. By maintaining this Li₂S to P₂S₅ ratio within this range, the lithium-ion conductivity can be increased. The lithium-ion conductivity of the sulfide-based solid electrolyte is preferably 1 × 10⁻⁶. -4 S / cm or higher, more preferably 1×10-3 S / cm or higher.
[0180] Examples of such compounds include, for instance, compounds derived from a composition of sulfides containing Li₂S and elements from Groups IIIA to VA. Specific examples include Li₂S-P₂S₅, Li₂S-GeS₂, Li₂S-GeS₂-ZnS, Li₂S-Ga₂S₃, Li₂S-GeS₂-Ga₂S₃, Li₂S-GeS₂-P₂S₅, Li₂S-GeS₂-Sb₂S₅, Li₂S-GeS₂-Al₂S₃, Li₂S-SiS₂, Li₂S-Al₂S₃, Li₂S-SiS₂-Al₂S₃, Li₂S-SiS₂-P₂S₅, Li₂S-SiS₂-LiI, Li₂S-SiS₂-Li₄SiO₄, Li₂S-SiS₂-Li₃PO₄, and Li₂S-P₂S₅. 10 GeP2S 12 Among them, crystalline and / or amorphous raw material compositions consisting of Li2S-P2S5, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-SiS2-P2S5, Li2S-SiS2-Li4SiO4, and Li2S-SiS2-Li3PO4 are preferred due to their high lithium-ion conductivity.
[0181] As a method for synthesizing sulfide-based solid electrolytes using such a raw material composition, an amorphization method can be cited as an example. Examples of amorphization methods include mechanical grinding and melt quenching. Among these, mechanical grinding is preferred because it can be performed at room temperature, simplifying the manufacturing process.
[0182] Sulfide-based solid electrolytes can be synthesized, for example, by referring to the literature such as T. Ohtomo, A. Hayashi, M. Tatsumisago, Y. Tsuchida, S. Hama, K. Kawamoto, Journal of Power Sources, 233, (2013), pp231-235 or A. Hayashi, S. Hama, H. Morimoto, M. Tatsumisago, T. Minami, Chem. Lett., (2001), pp872-873.
[0183] <Oxide-based solid electrolytes>
[0184] Oxide-based solid electrolytes preferably contain oxygen atoms (O) and metal elements from Group IA or Group IIA of the periodic table, possessing both ionic conductivity and electronic insulation. Examples of such oxide-based solid electrolytes include Li. xa Laya TiO3 [xa=0.3~0.7, ya=0.3~0.7] (LLT), Li7La3Zr2O 12 (LLZ), Li with a LISICON (lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4 and LiTi2P3O with a NASICON (sodium superionic conductor) crystal structure 12 Li (1+xb+yb) (Al, Ga) xb (Ti, Ge) (2-xb) Si yb P (3-yb) O 12 (where 0≤xb≤1, 0≤yb≤1), Li7La3Zr2O with a garnet-type crystal structure 12 .
[0185] Furthermore, as an oxide-based solid electrolyte, phosphorus compounds containing Li, P, and O are preferred. Examples include lithium phosphate (Li3PO4), LiPON (in which a portion of the oxygen atom of lithium phosphate is replaced by a nitrogen atom), and LiPOD (where D represents at least one selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, and Au). Additionally, LiAON (where A represents at least one selected from Si, B, Ge, Al, C, and Ga) is also preferred.
[0186] Among them, Li (1+xb+yb) (Al, Ga) xb (Ti, Ge) (2-xb) Si yb P (3-yb) O 12 (Where 0≤xb≤1, 0≤yb≤1) Due to their high lithium-ion conductivity, stable chemical properties, and ease of handling, they are preferred. They can be used alone or in combination of two or more.
[0187] The preferred lithium-ion conductivity of oxide-based solid electrolytes is 1×10⁻⁶. -6 S / cm or higher, more preferably 1×10 - 5 S / cm or higher, with a particularly preferred value of 5×10⁻⁶. -5 S / cm or higher.
[0188] 3.3. Other additives
[0189] In addition to the components described above, the all-solid-state secondary battery slurry of this embodiment may also contain other additives as needed. Examples of other additives include conductivity imparting agents, thickeners, and liquid media (excluding components introduced from the all-solid-state secondary battery binder composition).
[0190] <Conductive agent>
[0191] Conductivity-improving agents have the effect of enhancing electronic conductivity and are therefore added to all-solid-state slurries for secondary batteries used to form positive or negative electrode active material layers. Specific examples of conductivity-improving agents include activated carbon, acetylene black, Ketjen black, furnace black, graphite, carbon fiber, fullerene, and other carbons. Among these, acetylene black and furnace black are preferred. When the all-solid-state slurry for secondary batteries in this embodiment contains a conductivity-improving agent, the proportion of the conductivity-improving agent relative to 100 parts by weight of the active material is preferably 20 parts by weight or less, more preferably 1 to 15 parts by weight, and particularly preferably 2 to 10 parts by weight.
[0192] <Thickener>
[0193] Specific examples of thickeners include the thickeners listed in the "2.2. Other Additives" section on "Thickeners" above. When the all-solid secondary battery slurry of this embodiment contains a thickener, the proportion of the thickener relative to 100 parts by weight of all solid components of the all-solid secondary battery slurry is preferably 5 parts by weight or less, and more preferably 0.1 to 3 parts by weight.
[0194] <Liquid Medium>
[0195] As a specific example of a liquid medium, the liquid medium exemplified in section "2.1. Liquid Medium (B)" above can be cited. When adding a liquid medium to the all-solid-state secondary battery slurry of this embodiment, the same liquid medium (B) contained in the all-solid-state secondary battery binder composition can be added, or a different liquid medium can be added; preferably, the same liquid medium is added. In order to ensure good coatability and suppress the concentration gradient of the conjugated diene copolymer (A) and the active material during the drying process after coating, the content ratio of the liquid medium in the all-solid-state secondary battery slurry of this embodiment can be adjusted to any ratio.
[0196] 3.4. Preparation method of slurry for all-solid-state secondary batteries
[0197] The all-solid secondary battery slurry of this embodiment can be manufactured by any method as long as it contains the above-mentioned all-solid secondary battery binder composition and solid electrolyte.
[0198] However, to manufacture a slurry with better dispersibility and stability more efficiently and cheaply, it is preferable to manufacture it by adding a solid electrolyte and any additives as needed to the above-mentioned all-solid-state secondary battery binder composition and mixing them. The mixing of the all-solid-state secondary battery binder composition with the other components can be carried out using stirring based on known methods.
[0199] As a mixing method for manufacturing slurries for all-solid-state secondary batteries, it is necessary to select a mixer capable of mixing to the point where no solid electrolyte particle agglomerates remain in the slurry, and to obtain necessary and sufficient dispersion conditions. The degree of dispersion can be measured using a particle size analyzer, and preferably, the mixture is dispersed to the point where at least no agglomerates larger than 100 μm are present. Examples of mixers suitable for such conditions include ball mills, bead mills, sand mills, deaerators, pigment dispersers, pulverizers, ultrasonic dispersers, homogenizers, planetary mixers, Hobart mixers, etc.
[0200] The preparation of the slurry for all-solid-state secondary batteries (the mixing operation of the components) is preferably carried out under reduced pressure at least a part of the process. This prevents the formation of bubbles in the resulting positive electrode active material layer, negative electrode active material layer, or solid electrolyte layer. The degree of reduced pressure, in absolute pressure, is preferably 5.0 × 10⁻⁶. 3 ~5.0×10 5 Approximately Pa.
[0201] 4. Solid electrolyte tablets
[0202] One embodiment of the present invention provides a solid electrolyte sheet having a layer formed by coating a substrate with the aforementioned all-solid secondary battery slurry and drying it.
[0203] The solid electrolyte sheet of this embodiment can be manufactured, for example, by applying the above-mentioned all-solid secondary battery slurry onto a film serving as a substrate using a scraping method (e.g., blade method), calendering method, spin coating method, dip coating method, inkjet printing method, gravure printing method, mold coating method, or spray coating method, and then drying it to form a layer, and then peeling off the film. As such a film, for example, a general film such as a PET film that has undergone a demolding treatment can be used.
[0204] Alternatively, a slurry for all-solid secondary batteries containing a solid electrolyte can be directly coated onto the surface of the raw sheet of the object to which the solid electrolyte sheet is stacked or other components of an all-solid secondary battery, and then dried to form a solid electrolyte sheet.
[0205] In this embodiment, the solid electrolyte sheet is preferably coated with the aforementioned all-solid-state secondary battery slurry with a layer thickness preferably in the range of 1 to 500 μm, more preferably 1 to 100 μm. If the layer thickness is within the above range, conductive ions such as lithium ions become easier to migrate, thus increasing the battery output. In addition, if the layer thickness is within the above range, the overall thickness of the battery can be reduced, thus increasing the capacity per unit volume.
[0206] There are no particular limitations on the drying of slurry for all-solid-state secondary batteries; any method such as heat drying, vacuum drying, or heat-vacuum drying can be used. There are no particular limitations on the drying atmosphere; for example, it can be carried out in an atmospheric atmosphere.
[0207] When a solid electrolyte sheet contains both a positive electrode active material and a solid electrolyte, it functions as a positive electrode active material layer. When a solid electrolyte sheet contains both a negative electrode active material and a solid electrolyte, it functions as a negative electrode active material layer. Furthermore, when a solid electrolyte sheet contains only a solid electrolyte and not both a positive and negative electrode active material, it functions as a solid electrolyte layer.
[0208] 5. Electrodes for all-solid-state secondary batteries and all-solid-state secondary batteries
[0209] An all-solid-state secondary battery electrode according to one embodiment of the present invention includes a current collector and an active material layer formed by coating the surface of the current collector with the all-solid-state secondary battery slurry and drying it. The all-solid-state secondary battery electrode can be manufactured by coating the surface of a current collector such as a metal foil with the all-solid-state secondary battery slurry to form a coating film, and then drying the coating film to form an active material layer. Because the all-solid-state secondary battery electrode manufactured in this way is formed by bonding an active material layer containing the conjugated diene copolymer (A), a solid electrolyte, and an active material, as well as any components added as needed, onto the current collector, it exhibits excellent flexibility, abrasion resistance, and anti-dust properties, and demonstrates good charge-discharge durability characteristics.
[0210] As current collectors for both the positive and negative electrodes, electron conductors that do not cause chemical changes are preferred. For the positive electrode current collector, aluminum, stainless steel, nickel, titanium, and their alloys are preferred, as are current collectors made by treating the surface of aluminum or stainless steel with carbon, nickel, titanium, or silver; aluminum or aluminum alloys are more preferred. For the negative electrode current collector, aluminum, copper, stainless steel, nickel, titanium, and their alloys are preferred, as are aluminum, copper, and copper alloys.
[0211] The shape of the current collector is typically a film-shaped current collector, but mesh, die-cut shapes, slats, porous bodies, foams, and molded fiber bodies are also acceptable. The thickness of the current collector is not particularly limited, but is preferably 1 μm to 500 μm. Furthermore, the surface of the current collector is preferably given an uneven texture through surface treatment.
[0212] Methods for coating the slurry for all-solid-state secondary batteries onto the current collector can include doctor blade method, reverse roller method, comma method, gravure method, or air knife method. For the drying conditions of the coated film of the slurry for all-solid-state secondary batteries, the processing temperature is preferably 20–250°C, more preferably 50–150°C, and the processing time is preferably 1–120 minutes, more preferably 5–60 minutes.
[0213] Alternatively, the active material layer formed on the current collector can be compressed by pressing. As a pressing method, high-pressure ultra-pressing, soft presses, 1-ton presses, etc., can be used. The pressing conditions can be appropriately set according to the processing machine used.
[0214] For such an active material layer formed on a current collector, for example, the thickness is 40–100 μm and the density is 1.3–2.0 g / cm³. 3 .
[0215] The electrodes manufactured in this way are suitable for use as electrodes in all-solid-state secondary batteries, specifically as positive and / or negative electrodes for all-solid-state secondary batteries, in which a solid electrolyte layer is sandwiched between a pair of electrodes. Furthermore, the solid electrolyte layer formed using the aforementioned all-solid-state secondary battery slurry is suitable for use as a solid electrolyte layer in all-solid-state secondary batteries.
[0216] The all-solid-state secondary battery of this embodiment can be manufactured using known methods. Specifically, the manufacturing method is as follows.
[0217] First, a slurry for the positive electrode of an all-solid-state secondary battery, containing a solid electrolyte and a positive electrode active material, is coated onto a current collector and dried to form a positive electrode active material layer, thus fabricating the positive electrode for an all-solid-state secondary battery. Next, a slurry for a solid electrolyte of an all-solid-state secondary battery, containing a solid electrolyte, is coated onto the surface of the positive electrode active material layer of this positive electrode and dried to form a solid electrolyte layer. Similarly, a slurry for a negative electrode of an all-solid-state secondary battery, containing a solid electrolyte and a negative electrode active material, is coated onto the surface of the solid electrolyte layer and dried to form a negative electrode active material layer. Finally, a current collector (metal foil) on the negative electrode side is placed on the surface of this negative electrode active material layer, thereby obtaining the desired structure of an all-solid-state secondary battery.
[0218] Alternatively, a solid electrolyte sheet can be fabricated on a release PET film and bonded to a pre-fabricated positive or negative electrode for an all-solid-state secondary battery. Then, the release PET film is peeled off, thereby obtaining the desired all-solid-state secondary battery structure. It should be noted that conventional methods can be used for coating the above compositions. In this case, it is preferable to perform heat treatment after coating the all-solid-state secondary battery positive electrode slurry, the all-solid-state secondary battery solid electrolyte layer slurry, and the all-solid-state secondary battery negative electrode slurry. The heating temperature is preferably above the glass transition temperature of the conjugated diene copolymer (A). Specifically, it is preferably above 30°C, more preferably above 60°C, and most preferably above 100°C. The upper limit is preferably below 300°C, more preferably below 250°C. By heating within this temperature range, the shape of the conjugated diene copolymer (A) can be maintained while softening. Therefore, good adhesion and lithium-ion conductivity can be obtained in the all-solid-state secondary battery.
[0219] Furthermore, it is preferable to heat and pressurize simultaneously. The preferred pressurization pressure is 5 kN / cm². 2 The above, more preferably 10 kN / cm 2 The above is particularly preferred, with 20 kN / cm. 2 The above should be noted. In this specification, discharge capacity refers to the value relative to the weight of electrode active material, and in a half-cell, it is shown as the value relative to the weight of negative electrode active material.
[0220] 6. Example
[0221] The present invention will now be specifically described based on embodiments, but the present invention is not limited to these embodiments. Unless otherwise specified, "parts" and "%" in the embodiments and comparative examples refer to quality standards.
[0222] 6.1. Methods for determining various physical properties
[0223] In the following examples and comparative examples, the methods for determining each physical property value are as follows.
[0224] (1) Determination of 1,2-ethylene bond content
[0225] The 1,2-ethylene bond content (in mol%) in the polymer was determined using deuterated chloroform as a solvent and at 500 MHz. 1 It can be determined by H-NMR.
[0226] (2) Bonded styrene content
[0227] The bonded styrene content (in %) in the polymer was determined using deuterated chloroform as a solvent and at 500 MHz. 1 It can be determined by H-NMR.
[0228] (3) Weight-average molecular weight (Mw)
[0229] The retention time corresponding to the apex of the maximum peak of the GPC curve obtained using gel permeation chromatography (GPC) (trade name "HLC-8120GPC", manufactured by Tosoh Corporation) is calculated using polystyrene conversion.
[0230] (GPC conditions)
[0231] ·Pillars: 2 pieces under the brand name "GMHXL" (manufactured by Tosoh Corporation)
[0232] Column temperature: 40℃
[0233] • Mobile phase: Tetrahydrofuran
[0234] • Flow rate: 1.0 ml / min
[0235] • Sample concentration: 10 mg / 20 ml
[0236] (4) Hydrogenation rate (%) and [α]
[0237] The hydrogenation rate (%) and [α] of the polymer were measured using deuterated chloroform as a solvent, utilizing 500 MHz. 1 It is obtained by H-NMR. It should be noted that [α] is the value represented by the above mathematical expression (i).
[0238] (5) Energy storage elastic modulus (G') and loss tangent (tanδ)
[0239] The polymer was dissolved in xylene and dried at 40°C for 24 hours to prepare a uniform film with a thickness of 1.0 ± 0.3 mm. This film was then dried in a vacuum dryer at 160°C for 30 minutes. The film was removed from the vacuum dryer and cut into 10 mm × 10 mm strips, which were used as samples for measurement. Next, using a dynamic viscoelasticity measuring apparatus (Anton Paar, model "MCR 301"), the samples were fixed with parallel plates (product name "PP-12") and the dynamic viscoelasticity was measured under shear mode, a measurement temperature of 25°C, a frequency of 0.1 Hz, and a strain of 1%, obtaining the storage modulus and loss tangent values.
[0240] 6.2. Synthesis Examples of Conjugated Diene Copolymers
[0241] <Synthesis of Hydrogenation Catalyst E>
[0242] The hydrogenation catalyst E used in the following synthesis examples 9 and 10 is synthesized as follows.
[0243] A 1L three-necked flask equipped with a stirrer and a dropping funnel was purged with dry nitrogen, and 200ml of anhydrous tetrahydrofuran and 0.2mol of tetrahydrofurfuryl alcohol were added. Then, a 0.2mol solution of n-butyllithium / cyclohexane was added dropwise to the three-necked flask at 15°C to carry out the reaction, yielding a tetrahydrofurfuryl alcohol solution of lithium tetrahydrofurfuryloxy.
[0244] Next, a 1L three-necked flask equipped with a stirrer and a dropping funnel was purged with dry nitrogen, and 49.8g (0.2 mol) of bis(n-5-cyclopentadienyl)titanium dichloride and 250ml of anhydrous tetrahydrofuran were added. Then, a tetrahydrofuran solution of lithium tetrahydrofurfuryloxydichloride obtained by the method described above was added dropwise over approximately 1 hour with stirring at room temperature. After approximately 2 hours, the reddish-brown liquid was filtered, and the insoluble portion was washed with dichloromethane.
[0245] The filtrate and washing solution were then combined, and the solvent was removed under reduced pressure to obtain the hydrogenation catalyst E [bis(n-cyclopentadienyl)titanium (tetrahydrofurfuryloxy)chloride] (also known as "[chlorobis(2,4-cyclopentadienyl)titanium(IV)tetrahydrofurfuryl alkoxide"]). It should be noted that the yield was 95%.
[0246] <Synthesis example 1>
[0247] 25 kg of cyclohexane as a hydrocarbon solvent, 500 g of tetrahydrofuran as a vinyl control agent, 1000 g of styrene, 3850 g of 1,3-butadiene, and 0.55 g of divinylbenzene (55% by mass purity) (as m- and p-divinylbenzene) were added to a nitrogen-replaced 50 L autoclave. After adjusting the temperature of the reactor contents to 10 °C, 50 mmol of n-butyllithium as a polymerization initiator was added to initiate polymerization. Polymerization was carried out under insulated conditions, with a maximum temperature of 85 °C. When the polymerization conversion reached 99% (26 minutes after polymerization initiation), 150 g of 1,3-butadiene was added, and polymerization was further carried out for 3 minutes. Then, 2.5 mmol of tin tetrachloride was added, and the reaction was carried out for 30 minutes. Finally, 44 mmol of N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane (BTADS) was added, and the reaction was carried out for another 30 minutes to obtain a polymer solution containing a modified conjugated diene copolymer.
[0248] 15 g of 2,6-di-tert-butyl-p-cresol was added to the obtained polymer solution, followed by stripping with hot water adjusted to pH 9 with sodium hydroxide to remove the solvent, yielding a modified conjugated diene copolymer. The modified conjugated diene copolymer was then dried using a hot roller heated to 110°C to obtain polymer (A-1). Polymer (A-1) has a 1,2-ethylene bond content of 56 mol%, a bonded styrene content of 20%, and a weight-average molecular weight (Mw) of 303 × 10⁻⁶. 3The energy storage elastic modulus (G') is 130×10. 3 Pa, the loss tangent (tanδ) is 0.198.
[0249] <Synthesis Example 2 to Synthesis Example 8, Synthesis Example 11, Synthesis Example 12>
[0250] The types and amounts of raw materials used are as described in Table 1. Otherwise, polymers (A-2) to (A-8), (A-11), and (A-12) were synthesized according to the synthesis method of Synthesis Example 1 described above. The physical properties of each polymer determined by the above method are shown in Table 1.
[0251] <Synthesis Example 9>
[0252] (Process 1)
[0253] 26 kg of cyclohexane, 60 g of tetrahydrofuran, 370 g of styrene, and 3264 g of 1,3-butadiene were added as hydrocarbon solvent to a nitrogen-replaced 50 L autoclave. After adjusting the temperature of the reactor contents to 45 °C, a cyclohexane solution containing n-butyllithium (39 mmol) was added to initiate polymerization. Polymerization was carried out under insulated conditions, with a maximum temperature reaching 80 °C. Once the polymerization conversion was confirmed to be 99%, 111 g of butadiene was added, and polymerization was further induced for 5 minutes. Then, 2 mmol of tin tetrachloride was added, and the reaction was continued for 10 minutes. Finally, 28 mmol of N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane (BTADS) was added, and the reaction was continued for 20 minutes.
[0254] (Process 2)
[0255] After heating the reaction solution obtained in step 1 to above 80°C and introducing hydrogen into the system, 3.2 g of diethylaluminum chloride, 2.4 g of hydrogenation catalyst E, and n-butyllithium (15 mmol) were added. The hydrogen pressure was maintained above 0.7 MPa, and hydrogen was supplied to carry out the reaction until the specified hydrogen accumulation value was reached. The reaction solution was then restored to room temperature and pressure and extracted from the reaction vessel to obtain a polymer solution. 15 g of 2,6-di-tert-butyl-p-cresol was added to the obtained polymer solution containing the hydrogenated conjugated diene copolymer. Next, an aqueous solution (temperature: 80°C) adjusted to pH 8.5 using ammonia as a pH adjuster was placed in a desolventizing tank. The above polymer solution was further added (in a ratio of 100 parts by mass of the above aqueous solution to 1000 parts by mass of the polymer solution). Stripping was performed for 2 hours at a liquid phase temperature of 95°C in the desolventizing tank (steam temperature: 190°C) to remove the solvent. The polymer (A-9) was then dried using a hot roller at a temperature of 110°C. The hydrogenation rate of polymer (A-9) is 60% (α = 0.60), and other physical properties are shown in Table 1.
[0256] <Synthesis Example 10>
[0257] By changing the hydrogen supply in step 2, polymerization and desolventizing were performed in the same manner as in Synthesis Example 9 above, yielding polymer (A-9). The hydrogenation rate of polymer (A-9) was 88% (α = 0.88), and other physical properties are shown in Table 1.
[0258] <Synthesis Example 13>
[0259] 25 kg of cyclohexane as a hydrocarbon solvent, 500 g of tetrahydrofuran as a vinyl control agent, 1000 g of styrene, and 3900 g of 1,3-butadiene were added to a nitrogen-replaced 50 L autoclave. After adjusting the temperature of the reactor contents to 10 °C, 50 mmol of n-butyllithium and 44 mmol of N-trimethylsilylpiperazine were added as polymerization initiators to initiate polymerization. Polymerization was carried out under insulated conditions, with a maximum temperature of 85 °C. When the polymerization conversion reached 99% (26 minutes after polymerization initiation), 100 g of 1,3-butadiene was added, and polymerization was further carried out for 3 minutes. Then, 44 mmol of N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane (BTADS) was added, and the reaction was carried out for 30 minutes to obtain a polymer solution containing a modified conjugated diene copolymer.
[0260] Add as to the obtained polymer solution 42.3 mmol of silicon tetrachloride was added as a generating agent, and the mixture was stirred for another 10 minutes. 15 g of 2,6-di-tert-butyl-p-cresol was added, followed by stripping with hot water to remove the solvent, yielding the modified conjugated diene copolymer. The modified conjugated diene copolymer was then dried using a hot roller heated to 110°C to obtain polymer (A-13). Polymer (A-13) had a 1,2-ethylene bond content of 56 mol%, a bonded styrene content of 20%, and a weight-average molecular weight (Mw) of 297 × 10⁻⁶. 3 The energy storage elastic modulus (G') is 221 × 10⁻⁶. 3 Pa, the loss tangent (tanδ) is 0.083.
[0261] 6.3. Example 1
[0262] 6.3.1. Preparation of the adhesive composition
[0263] The polymer (A-1) obtained in Synthesis Example 1 above, along with 400 ppm of IRGANOX 1520L and 200 ppm of SUMILIZER TP-D as anti-aging agents, were added to anisole as liquid medium (B). The mixture was stirred at 90°C for 3 hours to dissolve the polymer (A-1) and anti-aging agents in the anisole. The binder composition was then transferred to a three-necked flask, and under reduced pressure of 100 Torr, bubbling with dry nitrogen gas containing less than 25.0 mg / L of water vapor was performed at 90°C for 4 hours to prepare a binder composition with a residual moisture content reduced to 43 ppm. Next, the adhesive composition was passed through a cartridge filter (ADVANTEC, perfluoropolymer cartridge filter, product name "TCF-300-H5MF") with a filter membrane having an average pore size of 3.00 μm, and then through a magnetic filter (TOK Engineering, magnetic flux density 8000 Gauss) before being filled into a 1L HYPER PURE BOTTLE (multilayer barrier container for ultra-high purity solvents) commercially available from KODAMAPLASTICS Co., Ltd. The total solids content of the adhesive composition was 10.3% when the total volume was set at 100% by mass. It should be noted that this preparation was carried out in a dry room at room temperature of 25°C, a cleanliness level of ISO 14644-1 Class 7, and an indoor dew point of -40°C DP or lower.
[0264] 6.3.2. Preparation of slurry for all-solid-state secondary batteries
[0265] <Preparation of Slurry for Positive Electrode of All-Solid-State Secondary Batteries>
[0266] A slurry for the positive electrode of an all-solid-state secondary battery was prepared by mixing 70 parts by mass of LiCoO2 (average particle size: 10 μm) as the positive electrode active material, 30 parts by mass of sulfide glass composed of Li2S and P2S5 (Li2S / P2S5 = 75 mol% / 25 mol%, average particle size 5 μm) as the solid electrolyte, 2 parts by mass of acetylene black as the conductive additive, and 2 parts by mass of the binder composition prepared above based on the solid content. Anisole was further added as the liquid medium, and the solid content concentration was adjusted to 75%. The mixture was then stirred for 10 minutes using a rotary mixer (THINKY Corporation, Awatori Rentaro ARV-310) to prepare the slurry.
[0267] <Preparation of slurry for solid electrolyte layer in all-solid-state secondary batteries>
[0268] 100 parts by mass of a sulfide glass composed of Li2S and P2S5 (Li2S / P2S5 = 75 mol% / 25 mol%, average particle size 5 μm), which serves as a solid electrolyte, are mixed with 2 parts by mass of the binder composition prepared above, based on the solid content. Anisole is further added as a liquid medium, and the solid content concentration is adjusted to 55%. The mixture is then stirred for 10 minutes using a rotary mixer (THINKY Corporation, Awatori Rentaro ARV-310) to prepare a slurry for the solid electrolyte layer of an all-solid secondary battery.
[0269] <Preparation of slurry for negative electrode of all-solid-state secondary battery>
[0270] A slurry for an all-solid-state secondary battery negative electrode was prepared by mixing 65 parts by mass of artificial graphite (average particle size: 20 μm) as the negative electrode active material, 35 parts by mass of sulfide glass composed of Li2S and P2S5 (Li2S / P2S5 = 75 mol% / 25 mol%, average particle size 5 μm) as the solid electrolyte, and 2 parts by mass of the binder composition prepared above based on solid content. Anisole was further added as the liquid medium, and the solid content concentration was adjusted to 65%. The mixture was then stirred for 10 minutes using a rotary mixer (THINKY Corporation, Awatori Rentaro ARV-310) to prepare the slurry.
[0271] 6.3.3. Fabrication and Evaluation of the Positive and Negative Electrodes and Solid Electrolyte Layer in All-Solid-State Secondary Batteries
[0272] <Fabrication of the Positive Electrode of an All-Solid-State Secondary Battery>
[0273] The prepared all-solid secondary battery positive electrode was coated onto aluminum foil using a scraping method. The anisole was evaporated under reduced pressure at 120°C and dried for 3 hours, thereby producing an all-solid secondary battery positive electrode with a positive electrode active material layer of 0.1 mm thickness.
[0274] <Fabrication of Solid Electrolyte Layer>
[0275] The solid electrolyte slurry for the all-solid secondary battery prepared above was coated onto a demolded PET film using a doctor blade method. The anisole was evaporated under reduced pressure at 120°C and dried for 3 hours, thereby producing a solid electrolyte layer with a thickness of 0.1 mm.
[0276] <Fabrication of the negative electrode of an all-solid-state secondary battery>
[0277] The prepared all-solid secondary battery negative electrode was coated onto a stainless steel foil using a scraping method. The anisole was evaporated under reduced pressure at 120°C and dried for 3 hours, thereby producing an all-solid secondary battery negative electrode with a negative electrode active material layer of 0.1 mm thickness.
[0278] <Peel strength test of positive electrode of all-solid-state secondary battery>
[0279] For the positive electrode active material layer formed on aluminum foil in the above-mentioned all-solid-state secondary battery positive electrode, a 20 mm wide adhesive tape was attached to the positive electrode active material layer, and the peel strength was measured when it was peeled off at a peel angle of 90° and a peel speed of 50 mm / min. The evaluation criteria are as follows. The results are shown in Table 1 below.
[0280] (Evaluation Criteria)
[0281] AA: Peel strength is above 20 N / m.
[0282] A: Peel strength is above 10 N / m and less than 20 N / m.
[0283] B: Peel strength is above 5 N / m and less than 10 N / m.
[0284] C: Peel strength is less than 5 N / m.
[0285] <Flexibility Test of Positive Electrode in All-Solid-State Secondary Batteries>
[0286] The aluminum foil side of the positive electrode test piece was wound around a 1.0 mm diameter metal rod, and the presence of cracks in the positive electrode active material layer and damage at the winding end were evaluated. The evaluation criteria are as follows. The results are shown in Table 1 below. The absence of visible damage to the positive electrode active material layer indicates high flexibility of the test piece and good suitability for the all-solid-state secondary battery assembly process.
[0287] (Evaluation Criteria)
[0288] A: The positive electrode active material layer has no cracks, and the winding end is undamaged.
[0289] B: The positive electrode active material layer has no cracks, but there is damage at the winding end.
[0290] C: Cracks exist in the positive electrode active material layer.
[0291] <Determination of Lithium-ion Conductivity of Solid Electrolyte Layers>
[0292] The solid electrolyte layer peeled from the PET film was clamped in a unit consisting of two stainless steel plates and measured using an impedance analyzer. The lithium-ion conductivity was calculated from the Nyquist plot. The evaluation criteria are as follows. The results are shown in Table 1 below. A higher lithium-ion conductivity indicates a better all-solid-state secondary battery performance.
[0293] (Evaluation Criteria)
[0294] AA: Lithium-ion conductivity is 0.8 × 10⁻⁶-4 S / cm~1.0×10 -4 S / cm.
[0295] A: The lithium-ion conductivity is 0.5 × 10⁻⁶. -4 S / cm or higher and less than 0.8×10 -4 S / cm.
[0296] B: Lithium-ion conductivity is 0.2 × 10⁻⁶ -4 S / cm or higher and less than 0.5×10 -4 S / cm.
[0297] C: Lithium-ion conductivity less than 0.2 × 10⁻⁶ -4 S / cm.
[0298] 6.3.4. Fabrication and Evaluation of All-Solid-State Secondary Batteries
[0299] <Fabrication of an All-Solid-State Secondary Battery>
[0300] Cut a 13mm diameter circular plate from the positive electrode of the all-solid-state secondary battery prepared above, and cut a 15mm diameter circular plate from the negative electrode and the solid electrolyte layer peeled from the PET film. Next, attach the positive electrode of the all-solid-state secondary battery to one side of the solid electrolyte layer with the positive active material layer in contact with the solid electrolyte layer. Attach the negative electrode of the all-solid-state secondary battery to the other side of the solid electrolyte layer with the negative active material layer in contact with the solid electrolyte layer. Using a hot press, heat (120°C) and apply pressure (600MPa, 1 minute) to create a laminated body for an all-solid-state secondary battery with a stacked structure of aluminum foil / positive active material layer / solid electrolyte layer / negative active material layer / stainless steel foil. Then, insert this laminated body for an all-solid-state secondary battery into a 2032-type stainless steel coin-shaped casing containing gaskets and washers, and rivet the 2032-type coin-shaped casing together to manufacture the all-solid-state secondary battery.
[0301] <Cycle life characteristics (capacity retention)>
[0302] Using the all-solid-state secondary battery prepared above, charge-discharge tests were conducted at 30°C. Charge-discharge was measured at a rate of 0.1C within a potential range of 4.2V to 3.0V. Repeated charge-discharge cycles at this 0.1C rate were performed. The discharge capacity of the first cycle was set as A (mAh / g), and the discharge capacity of the 20th cycle was set as B (mAh / g). The capacity retention rate after 20 cycles was calculated using the following formula. The evaluation criteria are as follows. The results are shown in Table 1 below.
[0303] Capacity retention rate (%) after 20 cycles = (B / A) × 100
[0304] It should be noted that the C in the C-rate refers to the hourly rate, defined as (1 / X)C = rated capacity (Ah) / X (h). X represents the time required to charge or discharge the rated capacity. For example, 0.1C means the current value is rated capacity (Ah) / 10 (h).
[0305] (Evaluation Criteria)
[0306] AA: Capacity maintenance rate is 95%–100%.
[0307] A: Capacity maintenance rate is above 90% and below 95%.
[0308] B: Capacity maintenance rate is above 85% and below 90%.
[0309] C: Capacity maintenance rate is less than 85%.
[0310] <Yield Rate>
[0311] Using the all-solid-state secondary battery prepared above, 20 charge-discharge cycles were performed at a potential range of 4.2V to 3.0V at a rate of 0.1C within a 30°C environment. Then, a charge-discharge cycle was performed, charging to 4.2V at a rate of 0.1C at 0°C and discharging to 3.0V at a rate of 0.1C at 30°C. The presence of any abnormalities was evaluated according to the following criteria. The results are shown in Table 1 below. It should be noted that "abnormality" refers to a voltage drop of more than 0.1V during charging or discharging.
[0312] (Evaluation Criteria)
[0313] AA: 9 to 10 out of 10 all-solid-state secondary batteries can be charged and discharged without any abnormalities.
[0314] A: Of 10 all-solid-state secondary batteries, 7 to 8 can be charged and discharged without any abnormalities.
[0315] B: Of the 10 all-solid-state secondary batteries, 4 to 6 can be charged and discharged without any abnormalities.
[0316] C: Of the 10 all-solid-state secondary batteries, 0 to 3 can be charged and discharged without any abnormalities.
[0317] 6.4. Examples 2-11, Comparative Examples 1-2
[0318] The types and amounts of the components used are as described in Table 1 below. Apart from that, the binder composition, the all-solid secondary battery slurry, the all-solid secondary battery positive and negative electrodes, the solid electrolyte layer, and the all-solid secondary battery were prepared in the same manner as in Example 1 above, and evaluated.
[0319] 6.5. Evaluation Results
[0320] Table 1 below summarizes the composition, physical properties, and evaluation results of the polymers used in Examples 1-11 and Comparative Examples 1-2.
[0321] [Table 1]
[0322]
[0323] The abbreviations or product names in Table 1 above represent the following compounds.
[0324] <Modifier>
[0325] BTADS: N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane
[0326] Anti-aging agents
[0327] BHT: 2,6-di-tert-butyl-p-cresol
[0328] • IRGANOX 1520L: Manufactured by BASF JAPAN, 2-methyl-4,6-bis[(n-octylthio)methyl]phenol
[0329] ·SUMILIZER TP-D: Made by Sumitomo Chemical Co., Ltd., pentaerythritol tetrakis(3-dodecylthiopropionate)
[0330] <Liquid Medium (B)>
[0331] • DIBK: Diisobutyl ketone
[0332] Based on the results in Table 1 above, it was confirmed that when using the binders of Examples 1 to 11 and binder compositions containing the binders, it is possible to produce all-solid-state secondary batteries with excellent adhesion and flexibility, as well as excellent lithium-ion conductivity and cycle life characteristics and high yield.
[0333] It should be noted that in Examples 1 to 11, the slurry used as the electrode slurry for all-solid-state secondary batteries was a slurry containing an all-solid-state secondary battery binder composition, an active material, and a solid electrolyte. It was confirmed that in the active material layer formed from this slurry, when the peel strength was measured, there was no situation where the active material layer itself became brittle, resulting in the detachment or cracking of the active material or solid electrolyte; sufficient adhesion to the polymer was obtained between either the active material or the solid electrolyte. Therefore, it can be inferred that: the active material layer formed by using the all-solid-state secondary battery binder composition of the present invention has sufficient adhesion to the solid electrolyte layer; and, when the solid electrolyte layer is formed by using the all-solid-state secondary battery binder composition of the present invention, high workability is also obtained, and the formed solid electrolyte layer has sufficient adhesion to the active material layer.
[0334] This invention is not limited to the embodiments described above and can be modified in various ways. This invention includes configurations that are substantially the same as those described in the embodiments (e.g., configurations with the same function, method, and result, or configurations with the same purpose and effect). Furthermore, this invention includes configurations in which non-essential parts of the configurations described in the above embodiments are replaced with other configurations. Furthermore, this invention also includes configurations that achieve the same effect as those described in the above embodiments or that can achieve the same purpose. Furthermore, this invention also includes configurations in which known technology is incorporated into the configurations described in the above embodiments.
Claims
1. A binder for all-solid secondary batteries, comprising a conjugated diene copolymer (A). The conjugated diene-based copolymer (A) has an aromatic vinyl unit based on an aromatic vinyl compound and a conjugated diene unit based on a conjugated diene compound, and a storage elastic modulus G' measured at a measurement temperature of 25°C, a frequency of 0.1 Hz, and a strain of 1% using a dynamic viscoelasticity measuring device is 4.0 x 10 4 Pa to 2.0 x 10 5 Pa and a loss tangent tan δ is 0.10 to 0.
80. When the proportions of the structural units represented by formula (1), formula (2), formula (3), and formula (4) in the conjugated diene copolymer (A) are set as p, q, r, and s, respectively, the value α represented by the following mathematical formula (i) is less than 0.5, where, The composition ratio is a molar ratio. α=(p+(0.5×r)) / (p+q+(0.5×r)+s)・・・(i) 。 2. The all-solid-state binder for secondary batteries according to claim 1, wherein, The conjugated diene copolymer (A) has a bonded styrene content of 5-45%.
3. The all-solid-state binder for secondary batteries according to claim 1 or 2, wherein, The conjugated diene copolymer (A) has units based on a modifier containing at least one atom selected from nitrogen, oxygen, silicon, germanium and tin atoms.
4. A binder composition for an all-solid secondary battery, comprising the all-solid secondary battery binder of claim 1 and a liquid medium (B).
5. The binder composition for all-solid-state secondary batteries according to claim 4, wherein, The liquid medium (B) is selected from at least one of aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, ketones, esters and ethers.
6. The all-solid-state binder composition for secondary batteries according to claim 4 or 5 is formed by dissolving the conjugated diene copolymer (A) in the liquid medium (B).
7. A slurry for an all-solid secondary battery, comprising the all-solid secondary battery binder composition of claim 4 and a solid electrolyte.
8. The all-solid-state secondary battery slurry according to claim 7, wherein, The solid electrolyte contains a sulfide-based solid electrolyte or an oxide-based solid electrolyte.
9. An all-solid-state secondary battery, comprising at least a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer. At least one of the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer is a layer formed by coating and drying the slurry for the all-solid-state secondary battery as described in claim 7 or 8.
10. A solid electrolyte sheet for an all-solid-state secondary battery, comprising a layer formed by coating a slurry for an all-solid-state secondary battery as described in claim 7 or 8 onto a substrate and drying it.
11. A method for manufacturing a solid electrolyte sheet for an all-solid-state secondary battery, comprising the steps of coating the all-solid-state secondary battery slurry of claim 7 or 8 onto a substrate and drying it.
12. A method for manufacturing an all-solid-state secondary battery, comprising manufacturing an all-solid-state secondary battery by means of the method for manufacturing a solid electrolyte sheet for an all-solid-state secondary battery as described in claim 11.
Citation Information
Patent Citations
Riniamootano seigyohoshiki
JP1976020522A
JP1988004841B2
Olefin hydrogenation catalyst and hydrogenation of polymer using said catalyst
JP1989037970B2
Method for manufacturing solid electrolyte sheets
JP1995087045B2
Solid electrolyte mold, electrode mold and electrochemical element
JP1999086899A