A selective profile control agent and a preparation method thereof

By preparing selective modulators and using emulsion polymerization technology to form nano- and micro-sized and network particles, the problems of short gelation time and oil reservoir contamination of existing modulators have been solved. This has enabled selective blocking of water flow channels and deep modulators, thereby improving oilfield recovery.

CN116854849BActive Publication Date: 2026-11-24XIAN CHANGQING PETROCHEMICAL CORP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210314737.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2026-11-24
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

Existing modifiers have problems in oilfield development, such as short gelation time, oil layer contamination, difficulty in controlling foaming, weak modifier capability, and inability to selectively seal oil and water layers, resulting in rapid increase in water cut and low recovery rate in oil wells.

Method used

By preparing a selective water-blocking agent, an initiator is added after mixing the aqueous and oil phases to form an emulsion, which is then used to initiate polymerization and form nano-micro and network particles. This agent has selective water-blocking function, which can block water flow channels in high water-cut layers and dissolve in oil layers, thus achieving deep water-blocking.

Benefits of technology

It achieves selective blocking of water flow channels, improves oilfield recovery, avoids contamination of oil reservoirs, and has selective regulation and drive functions, effectively changing the direction of water flow to enter the deep reservoir.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a selective water-blocking agent and its preparation method. The selective water-blocking agent is formed by mixing an aqueous phase and an oil phase to form an emulsion, followed by adding an initiator to initiate polymerization. The aqueous phase comprises 31-52 parts by weight, and the oil phase comprises 48-69 parts by weight. The aqueous phase includes deionized water, Span, Tween 80, polyoxyethylene ether, oxidant, reducing agent, and azobisisobutyronitrile (AIBN). The oil phase includes a dispersant, monomer, oleic acid, maleic anhydride, and nano-silica. This selective water-blocking agent enters high-water-cut formations with injected water, forming physical blockages in fractures and pores within the porous medium. It contains a large number of lipophilic groups and a network structure. After injection into the formation, when encountering an aqueous layer, water molecules do not enter the network structure to cause swelling or dissolution; however, when encountering an oil layer, it dissolves without affecting the oil layer's permeability. Therefore, it is beneficial for waterflooding and improving oil recovery, exhibiting selective water-blocking function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of petroleum extraction technology, specifically relating to a selective modifier and its preparation method. Background Technology

[0002] As tertiary oil recovery progresses, the continuous advance of formation water or injected water leads to the sudden surge of water tongues in single-layer oilfields, resulting in a rapid increase in water cut in oil wells and low reservoir recovery rates. Currently, water injection well profile control is an important measure for oil well control and stable production. Most water injection modifiers are currently divided into two categories: gels and inorganic-organic particles. They alter the water absorption profile by blocking pores and fractures.

[0003] Currently, there are many types of displacement modifiers used both domestically and internationally, including viscoelastic weak gels, foams, and polymer microspheres. Relevant patents include: CN101712865A, entitled "A viscoelastic weak gel displacement modifier"; CN101314710, entitled "Foam displacement modifier, oil displacement system, and oil displacement method"; and CN102504793A, entitled "A core-shell polymer microsphere displacement modifier and its preparation method," etc. However, these modifiers have the following drawbacks or shortcomings in field applications: 1) Viscoelastic weak gel-type modifiers have short gelation times and are prone to forming blockages near the wellbore, failing to achieve the desired deep-layer modifier effect. Furthermore, while they may block water channeling, they easily contaminate oil-bearing and low-permeability layers, affecting post-treatment water injection and oil production operations, and in severe cases, even leading to the abandonment of oil and water wells. Foam-type modifiers suffer from difficulties in controlling foaming and foaming under formation conditions. Polymer microsphere-type modifiers have weak modifier capabilities and are unsuitable for high-porosity, high-permeability reservoirs.

[0004] 2) The injected modifier cannot selectively block the oil and water layers (i.e., block water but not oil), but blocks both oil and water layers together, causing some potential oil layers to be unable to start production. Summary of the Invention

[0005] The purpose of this invention is to provide a selective modulator that overcomes the aforementioned technical problems in the prior art.

[0006] Another object of the present invention is to provide a method for preparing a selective modulator, wherein a polymerization reaction occurs to form nano-micro and network particles.

[0007] Therefore, the technical solution provided by the present invention is as follows: A selective modulator is formed by mixing an aqueous phase and an oil phase to form an emulsion and then adding an initiator to initiate polymerization, wherein the weight parts of the aqueous phase are 31-52 parts and the weight parts of the oil phase are 48-69 parts. The aqueous phase includes deionized water, Span, Tween 80, polyoxyethylene ether, oxidant, reducing agent and azobisisobutyronitrile; the oil phase includes dispersant, monomer, oleic acid, maleic anhydride and nano silica.

[0008] The weight proportions of each component in the aqueous phase are as follows: 400-700 parts deionized water, 50-150 parts Span, 100-130 parts Tween 80, 100-300 parts polyoxyethylene ether, 10-30 parts oxidant, 5-10 parts azobisisobutyronitrile, and 5-10 parts reducing agent.

[0009] The weight parts of each component in the oil phase are as follows: 400-600 parts of dispersant, 150-200 parts of monomer, 50-300 parts of oleic acid, 50-100 parts of maleic anhydride, and 50-100 parts of nano-silica.

[0010] The span is either span 60 or span 80.

[0011] The reducing agent is ferrous sulfate or sodium metabisulfite.

[0012] The oxidant is tert-butyl hydroperoxide or ammonium persulfate with a mass fraction of 40%.

[0013] The dispersant is diesel oil or white oil.

[0014] The monomer is styrene or propylenebenzene.

[0015] A method for preparing a selective modulator / deflector includes the following steps: Step 1) Add deionized water, Span, Tween 80, polyoxyethylene ether, oxidant and azobisisobutyronitrile to a container in sequence, and stir until homogeneous to obtain an aqueous phase; Step 2) Mix the dispersant, monomer, oleic acid, maleic anhydride and nano silica evenly to obtain the oil phase; Step 3) Place the well-stirred oil phase into a homogenizer, add the aqueous phase at a homogenization speed of 2000-6000 r / min, and homogenize for 25-30 min to obtain an emulsion. Step 4) At a stirring speed of 100-150 r / min, continuously purge the emulsion with nitrogen gas for 20-30 min; Step 5) After heating the emulsion to 28-30℃, add the reducing agent and simultaneously increase the stirring speed to 500-600 r / min; Step 6) After the emulsion temperature exceeds 60°C, reduce the rotation speed to 100-150 r / min and continue the reaction for 1-1.5 h to obtain a milky white liquid.

[0016] The beneficial effects of this invention are: The selective water-blocking agent provided by this invention possesses the characteristics of general selective materials. This selective water-blocking agent enters high-water-cut formations along with injected water. At fractures and pores, individual particles directly seal or multiple particles form a bridging structure, creating physical blockage in the porous medium and reducing the relative permeability of the aqueous phase. Simultaneously, this water-blocking agent contains a large number of lipophilic groups and has a network molecular structure. After injection into the formation, when encountering an aqueous layer, water molecules will not enter the network structure to cause swelling or dissolution; however, when encountering an oil layer, it will dissolve without affecting the oil layer's permeability. Therefore, it is beneficial for waterflooding to improve oil recovery and has the function of selective water-blocking.

[0017] The method of this invention involves homogenizing the aqueous and oil phases to form an O / W type emulsion, then adding a reducing agent and using emulsion polymerization to prepare a nano-micro selective plugging agent. After the plugging agent is injected into the formation at a mass fraction of 0.2% to 0.5%, it gradually accumulates and blocks the water flow channels as the injected water enters the formation, changes the water flow direction, and gradually enters the deep part of the oil reservoir. After encountering the crude oil, it dissolves, thereby achieving the purpose of deep displacement.

[0018] The following will provide a more detailed explanation. Detailed Implementation

[0019] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification.

[0020] Exemplary embodiments of the present invention are now described; however, the present invention may be embodied in many different forms and is not limited to the embodiments described herein. These embodiments are provided to fully and completely disclose the invention and to fully convey its scope to those skilled in the art. The terminology used in the exemplary embodiments is not intended to limit the invention.

[0021] Unless otherwise stated, the terms used herein (including technical terms) have their common meaning as understood by one of ordinary skill in the art. Furthermore, it is understood that terms defined in commonly used dictionaries should be understood to have a meaning consistent with the context of their relevant field, and not to be interpreted as having an idealized or overly formal meaning.

[0022] Example 1: This embodiment provides a selective modulator, which is formed by mixing an aqueous phase and an oil phase to form an emulsion and then adding an initiator to initiate polymerization, wherein the weight parts of the aqueous phase are 31-52 parts and the weight parts of the oil phase are 48-69 parts. The aqueous phase includes deionized water, Span, Tween 80, polyoxyethylene ether, oxidant, reducing agent and azobisisobutyronitrile; the oil phase includes dispersant, monomer, oleic acid, maleic anhydride and nano silica.

[0023] This invention utilizes emulsion polymerization to prepare nano- and micro-sized selective plugging agents. After injection into the formation, these agents gradually accumulate and block water flow channels as the injected water enters the formation, altering the water flow direction and allowing it to penetrate deeper into the reservoir. Upon encountering crude oil, the plugging agent dissolves, achieving the purpose of deep reservoir regulation and displacement. The use of deionized water is to prevent chloride ions and other contaminants from affecting polymer formation during the polymerization process.

[0024] Example 2: Based on Example 1, this example provides a selective deflection agent, wherein the weight parts of each component in the aqueous phase are as follows: 400-700 parts of deionized water, 50-150 parts of Span, 100-130 parts of Tween 80, 100-300 parts of polyoxyethylene ether, 10-30 parts of oxidant, 5-10 parts of azobisisobutyronitrile, and 5-10 parts of reducing agent.

[0025] The weight parts of each component in the oil phase are as follows: 400-600 parts of dispersant, 150-200 parts of monomer, 50-300 parts of oleic acid, 50-100 parts of maleic anhydride, and 50-100 parts of nano-silica.

[0026] The span is either span 60 or span 80.

[0027] The reducing agent is ferrous sulfate or sodium metabisulfite.

[0028] The oxidant is tert-butyl hydroperoxide or ammonium persulfate with a mass fraction of 40%.

[0029] The dispersant is diesel oil or white oil.

[0030] The monomer is styrene or propylenebenzene.

[0031] Example 3: Based on Example 2, this example provides a selective displacement agent, wherein the weight parts of the aqueous phase and the oil phase are 50 parts and 50 parts respectively, wherein the aqueous phase comprises the following substances in parts by weight: The ingredients are: 410 parts deionized water, 150 parts Span, 100 parts Tween 80, 300 parts polyoxyethylene ether, 30 parts oxidant, 10 parts azobisisobutyronitrile, and 10 parts reducing agent. The relative molecular weight of the polyoxyethylene ether ranges from 400 to 500.

[0032] The oil phase comprises the following substances in parts by weight: 400 parts dispersant, 150 parts monomer, 300 parts oleic acid, 100 parts maleic anhydride, and 50 parts nano silica.

[0033] In this embodiment, Span is Span 60, the reducing agent is ferrous sulfate, the oxidizing agent is tert-butyl hydroperoxide, the dispersant is diesel oil, and the monomer is styrene.

[0034] The preparation process includes the following steps: Step 1) Add the prescribed amounts of deionized water, Span, Tween 80, polyoxyethylene ether, oxidant and azobisisobutyronitrile to a container in sequence, and stir until homogeneous to obtain an aqueous phase; Step 2) Mix the prescribed amounts of dispersant, monomer, oleic acid, maleic anhydride and nano silica evenly to obtain the oil phase; Step 3) Place the well-stirred oil phase into a homogenizer, add the aqueous phase at a homogenization speed of 2000-6000 r / min, and homogenize for 25-30 min to obtain an emulsion. Step 4) At a stirring speed of 100-150 r / min, continuously purge the emulsion with nitrogen gas for 20-30 min; Step 5) After heating the emulsion to 28-30℃, add the reducing agent and simultaneously increase the stirring speed to 500-600 r / min; Step 6) After the emulsion temperature exceeds 60°C, reduce the rotation speed to 100-150 r / min and continue the reaction for 1-1.5 h to obtain a milky white liquid.

[0035] Principle of this invention: In the aqueous phase, water, Span, Tween 80, and polyoxyethylene ether are physically stirred to form a homogeneous aqueous phase. In the oil phase, dispersant, monomer, and oleic acid are physically stirred and dissolved to form an oil phase. The oil and aqueous phases are then mixed together and stirred to form an emulsion. An initiator is then added to initiate polymerization, causing the unsaturated double bonds in the emulsion to undergo addition reactions, forming nano- and micro-sized network particles. Span, Tween, and polyoxyethylene ether act as emulsifiers in the oil and water phases, working synergistically to form a relatively stable microemulsion system. In the oil phase, monomer, oleic acid, and maleic anhydride serve as polymerizable materials, forming cross-linked network particles after the addition of the initiator.

[0036] Example 4: Based on Example 2, this example provides a selective displacement agent, wherein the weight parts of the aqueous phase and the oil phase are 45.6 parts and 48 parts, respectively, wherein the aqueous phase comprises the following substances in parts by weight: The ingredients are: 650 parts deionized water, 50 parts Span, 130 parts Tween 80, 100 parts polyoxyethylene ether, 10 parts oxidant, 5 parts azobisisobutyronitrile, and 5 parts reducing agent. The relative molecular weight of the polyoxyethylene ether ranges from 400 to 500.

[0037] The oil phase comprises the following substances in parts by weight: 600 parts dispersant, 200 parts monomer, 50 parts oleic acid, 50 parts maleic anhydride, and 100 parts nano silica.

[0038] The preparation process is the same as in Example 3.

[0039] In this embodiment, Span is Span 80, the reducing agent is sodium metabisulfite, the oxidizing agent is ammonium persulfate with a mass fraction of 40%, the dispersant is white oil, and the monomer is propylene benzene.

[0040] Example 5: Based on Example 2, this example provides a selective displacement agent, wherein the weight parts of the aqueous phase and the oil phase are 44.5 parts and 50 parts, respectively, wherein the aqueous phase comprises the following substances in parts by weight: The ingredients are: 500 parts deionized water, 100 parts Span, 120 parts Tween 80, 240 parts polyoxyethylene ether, 20 parts oxidant, 10 parts azobisisobutyronitrile, and 10 parts reducing agent. The relative molecular weight of the polyoxyethylene ether ranges from 400 to 500.

[0041] The oil phase comprises the following substances in parts by weight: 450 parts dispersant, 150 parts monomer, 250 parts oleic acid, 80 parts maleic anhydride, and 70 parts nano silica.

[0042] The preparation process is the same as in Example 3.

[0043] In this embodiment, Span is Span 60, the reducing agent is sodium metabisulfite, the oxidizing agent is tert-butyl hydroperoxide, the dispersant is diesel oil, and the monomer is propylene benzene.

[0044] Example 6: Based on Example 2, this example provides a selective displacement agent, wherein the weight parts of the aqueous phase and the oil phase are 35 parts and 50 parts, respectively, wherein the aqueous phase comprises the following substances in parts by weight: The ingredients are: 400 parts deionized water, 60 parts Span, 100 parts Tween 80, 120 parts polyoxyethylene ether, 10 parts oxidant, 10 parts azobisisobutyronitrile, and 5 parts reducing agent. The relative molecular weight of the polyoxyethylene ether ranges from 400 to 500.

[0045] The oil phase comprises the following substances in parts by weight: 500 parts dispersant, 180 parts monomer, 170 parts oleic acid, 70 parts maleic anhydride, and 80 parts nano silica.

[0046] The preparation process is the same as in Example 3.

[0047] In this embodiment, Span is Span 80, the reducing agent is ferrous sulfate, the oxidizing agent is ammonium persulfate with a mass fraction of 40%, the dispersant is white oil, and the monomer is styrene.

[0048] To further illustrate the effects of this invention, the performance of the selective relocation agents prepared in Examples 3-6 was tested and compared with that of polyacrylamide-based microgel relocation agents (comparative examples). The test results are shown in Table 1. The preparation method of the polyacrylamide-based microgel relocation agent involves dissolving monomers such as acrylamide in water, adding an initiator, heating and polymerizing to form a gel block, and then using a colloid mill or other granulation equipment to produce a product with micron-sized particles.

[0049] 1. Particle size measurement: A Malvern laser particle size analyzer was used for measurement based on the principle of dynamic light scattering. The particle size was measured after dispersion in solvents such as diesel fuel.

[0050] 2. Oil and water solubility measurements: The selective water plugging agent was centrifuged to separate the effective substances, which were then placed in kerosene and deionized water respectively and stirred for 48 hours. The mixture was then filtered using medium-speed quantitative filter paper, dried, and weighed to calculate its oil and water solubility. For oil solubility testing, the agent was placed in kerosene for 48 hours (25℃) for measurement; for water solubility testing, the agent was placed in deionized water for 48 hours (25℃) for measurement.

[0051] 3. Elongation: The separated effective material is processed a second time, then cut into strips of a certain size with a cutter, and its elongation is tested with a tensile tester.

[0052] Table 1 Technical Specifications of Optimizing and Depressing Agents Small particle size (50-200nm) is a prerequisite for selective water shut-off agents to penetrate deep into the formation. Oil solubility and water solubility are important technical indicators and theoretical support data for selective water shut-off. Elongation is a strength technical indicator to ensure that the selective water shut-off agent can block water flow channels.

[0053] The test results show that, compared with polyacrylamide-based microgel flood control agents, the selective flood control agent of this invention has the following advantages: firstly, smaller particle size, allowing it to effectively enter the formation with injected water; secondly, it is oil-soluble but water-insoluble, exhibiting selective flood control function and effectively blocking water flow channels; and thirdly, a high elongation rate of over 200%, resulting in high sealing strength and effective sealing of water flow pores. Furthermore, in laboratory evaluations, subsequent oil injection effectively released the seal without affecting the permanent seal.

[0054] The selective water-blocking agent of this invention, injected into the formation at a mass percentage of 0.2-0.5%, enters the high-water-cut layer as water is injected. At fractures and pores, individual particles directly seal or multiple particles form a bridging structure, creating physical blockage in the porous medium and reducing the relative permeability of the water phase. Simultaneously, this modifier contains a large number of lipophilic groups and has a network molecular structure. After injection into the formation, when encountering a water layer, water molecules will not enter the network structure to cause swelling or dissolution; however, when encountering an oil layer, it will dissolve without affecting the oil layer's permeability.

[0055] The above examples are merely illustrative of the present invention and do not constitute a limitation on the scope of protection of the present invention. All designs that are the same as or similar to the present invention are within the scope of protection of the present invention.

Claims

1. A selective deflector, characterized in that, The selective modulator is formed by polymerizing an emulsion of an aqueous phase and an oil phase, wherein the weight parts of the aqueous phase and the oil phase are 44.5 parts and 50 parts, respectively. The aqueous phase comprises the following components in parts by weight: 500 parts deionized water, 100 parts Span, 120 parts Tween 80, 240 parts polyoxyethylene ether, 20 parts tert-butyl hydroperoxide, 10 parts azobisisobutyronitrile, and 10 parts sodium metabisulfite; wherein the Span is Span 60, and the polyoxyethylene ether has a relative molecular weight range of 400-500. The oil phase comprises the following components in parts by weight: 450 parts diesel oil, 150 parts acrylonitrile, 250 parts oleic acid, 80 parts maleic anhydride, and 70 parts nano-silica. The selective retarder is prepared by the following process: Deionized water, Span 60, Tween 80, polyoxyethylene ether, tert-butyl hydroperoxide, and azobisisobutyronitrile are stirred until homogeneous to obtain an aqueous phase; diesel oil, acrylonitrile, oleic acid, maleic anhydride, and nano-silica are mixed and stirred until homogeneous to obtain an oil phase; the homogeneous oil phase is placed in a homogenizer, and the aqueous phase is added at a homogenization speed of 2000-6000 r / min, wherein the weight ratio of the aqueous phase to the oil phase is 44.5:50, and homogenized for 25-30 min to obtain an emulsion; nitrogen gas is continuously purged onto the emulsion at a stirring speed of 100-150 r / min for 20-30 min; sodium metabisulfite is added after the emulsion is heated to 28-30℃, and the stirring speed is increased to 500-600 r / min; after the emulsion temperature exceeds 60℃, the stirring speed is reduced to 100-150 r / min, and the reaction is continued for 1-1.5 h; The selective modulator has a particle size of 150 nm, a water solubility of 7%, and an oil solubility of 97%. The particle size was measured by dynamic light scattering and dispersion in diesel oil. The water solubility and oil solubility were measured by placing the separated effective substances in deionized water and kerosene at 25°C, stirring for 48 h, filtering, drying, and weighing.

2. The method for preparing a selective deflector according to claim 1, characterized in that, Includes the following steps: Step 1) Add the following parts by weight to a container in sequence: 500 parts deionized water, 100 parts Span 60, 120 parts Tween 80, 240 parts polyoxyethylene ether with a relative molecular weight range of 400-500, 20 parts tert-butyl hydroperoxide, and 10 parts azobisisobutyronitrile. Stir until homogeneous to obtain an aqueous phase. Step 2) Mix 450 parts diesel, 150 parts acrylbenzene, 250 parts oleic acid, 80 parts maleic anhydride and 70 parts nano silica in the following weight proportions to obtain an oil phase; Step 3) Take 44.5 parts of the aqueous phase and 50 parts of the oil phase, put the well-stirred oil phase into a homogenizer, add the aqueous phase at a homogenization speed of 2000-6000 r / min, and homogenize for 25-30 min to obtain an emulsion. Step 4) Under the condition of stirring speed of 100-150 r / min, continuously purge the emulsion with nitrogen gas for 20-30 min; Step 5) After heating the emulsion to 28-30℃, add 10 parts of sodium metabisulfite, and at the same time increase the stirring speed to 500-600 r / min; Step 6) After the emulsion temperature exceeds 60°C, reduce the rotation speed to 100-150 r / min and continue the reaction for 1-1.5 h to obtain a milky white liquid, which is the selective driving agent.

Citation Information

Patent Citations

  • Viscoelastic weak gel profile control agent

    CN101712865A

  • Core-shell polymer microsphere profile control and oil displacement agent and preparation method thereof

    CN102504793A

  • Polymer with selective water shutoff function, preparation method and application thereof

    CN109748992A

  • Oil-soluble latex blocking agent and preparation method thereof

    CN109762542A

  • Oil-soluble plugging agent as well as preparation method and application thereof

    CN114196385A