A Multi-parameter Quantitative Evaluation Method for Molten Steel Flow Field in Crystallizers Based on Mechanism Model
By establishing a multi-parameter quantitative evaluation method based on a mechanism model, the problem of lack of quantitative indicators in the existing technology is solved, and the direct evaluation and optimization of the effect of the molten steel flow field in the crystallizer on the defects of the billet are realized, thereby improving production efficiency and billet quality.
Patent Information
- Application Number
- CN202310786165.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-29
AI Technical Summary
Existing technologies lack direct quantitative indicators to evaluate the impact of the molten steel flow field in the crystallizer on defects in the cast billet, resulting in unclear directions for optimization and adjustment, making it difficult to improve the efficiency of continuous casting production.
A multi-parameter quantitative evaluation method based on a mechanism model is established. Through numerical simulation and flow field analysis, the influence of molten steel flow field on billet defects is quantified. A multi-parameter index value calculation formula is established for evaluating and optimizing process conditions or equipment structure.
It provides index values with clear theoretical basis, which can specifically evaluate and optimize defects in billets such as longitudinal cracks, corner transverse cracks, and inclusions in the billet shell, thereby improving production efficiency and billet quality.
Smart Images

Figure CN116861808B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a parameter quantification evaluation method, and more particularly to a multi-parameter quantification evaluation method for the flow field of molten steel in a crystallizer based on a mechanistic model. Background Technology
[0002] Billet defects are a significant factor affecting billet quality and continuous casting production efficiency. Optimizing production process parameters and the structure of equipment such as crystallizers or submerged entry nozzles (SENs) are the main methods to improve billet defects.
[0003] Current research methods often employ numerical simulations or water models to study the impact of various process conditions or structures on the molten steel flow field. For example, qualitative analysis is performed through flow field morphology, or the quality of the flow field is evaluated by comparing a single indirect parameter, failing to provide multi-parameter evaluation. For instance, the molten steel flow velocity at the crystallizer surface or the size of the molten steel circulation are used as indicators of flow field quality, but the correlation between these indicators and flow field quality is not clearly defined. Furthermore, the influence trends of these indicators are opposite for different common defects in cast billets, such as cracks and inclusions. Therefore, the evaluation methods used in previous studies are often vague and limited.
[0004] Further research methods, such as the F-number method, only describe a certain state of the molten steel flow field and obtain a numerical value without clear meaning. It is still necessary to define a better range through statistical analysis of practical data, which contradicts the original intention of the theoretical analysis stage.
[0005] In summary, current research methods lack a direct quantitative indicator to evaluate the impact of a specific process condition or structure on casting defects. They also fail to theoretically define the direction for optimization adjustments targeting a particular defect or to obtain the optimal value. Summary of the Invention
[0006] The technical objective of this invention is to address the shortcomings of the prior art by providing a multi-parameter quantitative evaluation method for the flow field of molten steel in a crystallizer based on a mechanistic model, so as to more accurately and effectively improve defects in continuously cast billets and increase the casting speed.
[0007] The technical solution of this invention to solve its technical problem is: a multi-parameter quantitative evaluation method for the flow field of molten steel in a crystallizer based on a mechanism model, characterized in that it includes:
[0008] S1. Establish a defect mechanism model for cast billets:
[0009] S1.1 Determine the cause and mechanism of the formation of a certain defect in a cast billet that needs to be studied;
[0010] S1.2 clarifies the influencing factors of the molten steel flow field on the cause of this defect among the above causes;
[0011] S2. Establish a steel flow field analysis model:
[0012] S2.1 Employs numerical simulation methods to establish analytical models of molten steel flow fields under different process conditions or equipment structures;
[0013] S2.2 Quantify the characteristics of the numerical simulation flow field, obtain the numerical simulation results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism;
[0014] S3. Establish a formula for calculating the parameter index value: Establish a formula for calculating the multi-parameter index value that can characterize the trend of this defect formation.
[0015] S4. Evaluation of Quantitative Index Value: Substitute the flow field quantitative parameter values under various relevant process conditions or equipment structures into the calculation formula obtained in S3 to obtain the quantitative index value of this defect under that condition.
[0016] Furthermore, the multiple parameters in S3 above refer to the calculation formula formed by multiple flow field-related parameters.
[0017] Furthermore, the quantitative index value obtained from S4 above is used to compare and analyze the advantages and disadvantages of different process conditions or equipment structures for a certain billet defect, and to analyze, study and optimize it.
[0018] Compared with the prior art, the present invention has the following outstanding advantages:
[0019] 1. Using the method of this invention, an index with theoretical basis and practical significance can be calculated for a certain defect in a casting billet. The calculated index value can be used to evaluate and analyze the process conditions or equipment structure.
[0020] 2. It is highly operable and can establish calculation models specifically for defects such as longitudinal cracks in the billet, transverse cracks at the corners, inclusions in the billet shell, and subcutaneous inclusions. Attached Figure Description
[0021] Figure 1 This is a diagram of the steel flow field trace of the present invention.
[0022] Figure 2 yes Figure 1 A partial view.
[0023] Figure 3 This is a line graph of the edge crack index C under different parameters in Embodiment 1 of the present invention.
[0024] Figure 4 This is a cloud map of the flow velocity at the surface of molten steel according to the present invention.
[0025] Figure 5 yes Figure 1A partial view.
[0026] Figure 6 This is a line graph of the subcutaneous inclusion index F under different parameters in Embodiment 2 of the present invention.
[0027] Figure 7 This is a schematic diagram of the SEN outlet structure in Embodiment 3 of the present invention.
[0028] Figure 8 yes Figure 7 Side view.
[0029] Figure 9 This is a line graph of the edge crack index C under different parameters in Embodiment 3 of the present invention. Detailed Implementation
[0030] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0031] For the purposes of the following detailed description, it should be understood that the invention may take various alternative variations and sequences of steps unless explicitly stated otherwise. Furthermore, except in any operational instance or where otherwise indicated, all figures representing quantities of ingredients as used, for example, in the specification and claims, should in all cases be understood to be modified by the term “about.” At least, and without attempting to limit the application of the principle of equivalents to the scope of the claims, each numerical parameter should be understood at least according to the number of significant figures reported and by applying common rounding techniques.
[0032] Although the numerical ranges and parameters illustrating the broad scope of the invention are approximate, the values described in the specific examples are reported as precisely as possible. However, any numerical value inherently contains some error that is necessarily caused by the standard deviation found in its corresponding test measurement.
[0033] It should also be understood that any range of values stated herein is intended to include all subranges included therein. For example, the range “1 to 10” is intended to include all subranges between (and including) the stated minimum value of 1 and the stated maximum value of 10, that is, a minimum value equal to or greater than 1 and a maximum value equal to or less than 10.
[0034] In this application, unless otherwise specified, the use of the singular includes the plural and the plural encompasses the singular. Additionally, in this application, unless otherwise expressly stated, the use of "or" means "and / or," even if "and / or" may be explicitly used in certain circumstances. Furthermore, in this application, unless otherwise specified, the use of "a" or "an" means "at least one / a." For example, "an" first material, "an" coating composition, etc., refer to one or more of any of these items.
[0035] This invention presents a multi-parameter quantitative evaluation method for the flow field of molten steel in a crystallizer based on a mechanistic model. It employs a quantitative index for evaluation, theoretically calculating the quantitative index value for a specific defect in the cast billet (e.g., transverse cracks, longitudinal cracks, surface depressions, surface inclusions, subcutaneous inclusions, etc.) under certain process conditions or equipment structures. This index is used to evaluate the effectiveness of addressing this defect under those conditions and to identify optimization directions or optimal values. This index is a relatively accurate, direct, and practically meaningful evaluation value.
[0036] The method of the present invention includes:
[0037] S1. Establish a defect mechanism model for cast billets.
[0038] S1.1 Determine the cause and mechanism of the formation of a certain defect in a cast billet that needs to be studied;
[0039] S1.2 clarifies the influencing factors of the molten steel flow field on the cause of this defect among the above causes.
[0040] S2. Establish a steel flow field analysis model.
[0041] S2.1 Employs numerical simulation methods to establish analytical models of molten steel flow fields under different process conditions or equipment structures.
[0042] S2.2 Quantify the characteristics of the numerical simulation flow field, obtain the numerical simulation results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism.
[0043] S3. Establish the formula for calculating the parameter index value.
[0044] Establish a multi-parameter index value calculation formula that can characterize the trend of this defect formation.
[0045] The aforementioned multi-parameter refers to a calculation formula formed by multiple flow field-related parameters, such as the flow distribution ratio, circulation size, liquid surface velocity, liquid surface height difference, liquid surface shear angle, etc. Different indices require corresponding parameter types.
[0046] S4. Evaluation of Quantitative Index Values
[0047] By substituting the flow field quantification parameter values under various relevant process conditions or equipment structures into the calculation formula obtained in S3, the quantification index value for this defect under that condition can be obtained.
[0048] This index value is used to compare and analyze the advantages and disadvantages of different process conditions or equipment structures for a certain billet defect, and to conduct analysis, research and optimization.
[0049] The aforementioned index value can be as high or as low as possible. It allows us to see how the index value changes after adjusting a certain condition. That is, it allows us to determine whether adjusting a certain condition theoretically improves or worsens the situation regarding this defect. It also considers index values for multiple defects, obtaining the optimal process conditions for billet quality and production efficiency after comprehensive analysis.
[0050] The main difference between this method and existing research methods, such as the F-number method, is that it can calculate a theoretically sound and practically meaningful numerical value for a specific defect in a cast billet, rather than a vague and meaningless value. It can specifically target defects such as longitudinal cracks, corner transverse cracks, inclusions in the billet shell, and subcutaneous inclusions, establishing computational models and using the calculated index values to evaluate and analyze process conditions or equipment structures, rather than providing a vague optimal range.
[0051] Example 1:
[0052] Taking a high-speed thin slab production line as an example, this quantitative evaluation method is used to evaluate different process parameters to address the problem of edge crack defects in the cast slab. This optimizes the production process, reduces casting defects, and improves production efficiency.
[0053] S1. Establish a defect mechanism model for cast billets.
[0054] S1.1 Determine the cause and mechanism of the formation of a specific defect in a cast billet that needs to be studied.
[0055] Based on previous research findings and analysis specific to this production line, the causes and mechanisms of edge crack defects in cast billets can be summarized into the following five aspects:
[0056] 1) The temperature in the edge area of the billet is higher, resulting in a thinner shell thickness at the edge.
[0057] 2) The temperature drop rate in the edge area of the billet shell is relatively slow, which causes uneven shrinkage of the billet shell, resulting in wrinkle deformation and uneven cooling of the billet shell;
[0058] 3) Sintering of protective slag at the meniscus of the edge causes wrinkles and deformation of the initial billet shell, resulting in uneven cooling of the billet shell;
[0059] 4) When the secondary cooling zone cools rapidly and the temperature distribution of the billet is uneven, it will generate greater stress;
[0060] 5) Abnormal steel composition, such as high carbon equivalent, will amplify the adverse effects of phase transformation in the material. Different regions will undergo phase transformation asynchronously, resulting in greater stress.
[0061] S1.2 clarifies the influencing factors of the molten steel flow field on the cause of this defect among the above-mentioned causes.
[0062] In the formation mechanism obtained in S1.1, the influencing factors of the molten steel flow field on the formation of this defect are extracted:
[0063] (1) The edge of the billet is hot and the thickness of the billet shell at the outlet of the crystallizer is thin, but the cooling speed is faster after entering the secondary cooling zone → resulting in low strength and high stress of the billet shell at the edge.
[0064] (2) The slow cooling of the edge shell makes the shrinkage rate of the edge area lower than that of other areas and forms wrinkles → resulting in uneven cooling of the edge shell, more structural defects, and greater internal stress.
[0065] In other words, the factors influencing the edge crack defects of the billet caused by the flow field of molten steel in the crystallizer are reduced to: ① high temperature in the edge region of the billet; ② relatively slow temperature drop rate in the edge region of the billet shell.
[0066] S2. Establish a steel flow field analysis model.
[0067] S2.1 Establish a steel flow field analysis model and obtain the flow field numerical simulation analysis results under different conditions.
[0068] To address the factors caused by the molten steel flow field within the crystallizer, a numerical simulation method was used to establish an analytical model of the molten steel flow field under different process conditions, which was then used to extract quantitative data.
[0069] In this embodiment, Fluent simulation analysis software is used to establish a numerical simulation analysis model (the calculation process, including model structure, mesh generation, algorithm settings, and boundary condition settings, is not detailed here). Through the simulation calculations performed by Fluent software, a flow field calculation result can be obtained for each set of process conditions, corresponding to a flow field trace diagram. This software is only one specific implementation method; other software can also be used to quantify the characteristics of the numerical simulation flow field.
[0070] Figure 1 This refers to the flow field trace diagram when the process conditions are continuous casting speed of 5.2 m / min, electromagnetic braking current intensity of 175 A, and SEN immersion depth of 170 mm.
[0071] S2.2 Quantify the characteristics of the numerical simulation flow field, obtain the numerical simulation results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism.
[0072] Based on the steel flow field analysis model established in S2.1, the quantitative values of the steel flow field distribution are extracted for further analysis and calculation, targeting the two defect causes related to the steel flow field in the crystallizer.
[0073] (1) Regarding the relatively high temperature at the edge of the billet, the main influencing factor is the proportion of molten steel flowing towards the edge region. The higher the proportion of molten steel flowing towards the edge, the higher the temperature in the edge region.
[0074] (2) Regarding the problem of relatively slow cooling at the edge of the billet, the main influencing factor is the ratio of upper and lower backflow formed after the molten steel reaches the edge. The larger the proportion of lower backflow, the smaller the temperature difference between the upper and lower parts of the billet shell in this area of the crystallizer, and the slower the cooling rate.
[0075] Therefore, it is necessary to extract the proportion of the flow stream flowing towards the edge and the proportion of the flow stream flowing backward from the edge from the flow field calculation results.
[0076] This embodiment obtains the numerical simulation results of the molten steel flow field under the required state by performing quantitative calculations using Fluent simulation analysis software. The specific method for obtaining the values is as follows ( Figure 2 for Figure 1 (Partial view):
[0077] 1) Point P is the point where the molten steel reaches the edge of the crystallizer after flowing out of SEN, where the flow velocity is the lowest. The value of D is the distance from point P to the liquid surface.
[0078] 2) Line a is located 0.2m above point P, that is, (D+0.2) is taken as the ordinate of line a. The velocity distribution of molten steel at line a is used to describe the circulation distribution in the flow field.
[0079] 3) Line b is located 0.2m below point P, that is, (D-0.2) is taken as the ordinate of line b. The steel velocity distribution at line b is used to describe the circulation distribution in the flow field.
[0080] 4) Obtain the proportion of molten steel flow in lines a and b, the proportion of flow towards the edge, and the reverse flow ratio of the edge flow by analyzing the molten steel flow velocity distribution values. This data acquisition method is standard in the industry and will not be elaborated upon here.
[0081] S3. Establish the multi-parameter exponent value calculation formula.
[0082] Analysis of the flow field trace diagram and the two influencing factors mentioned above shows that the larger the proportion of side flow, the higher the temperature at the edge of the billet. The larger the proportion of backflow in the edge region, the slower the cooling rate of the billet shell at the edge. Simultaneously, the edge temperature is directly proportional to the steel flow rate through the mold and inversely proportional to the cross-sectional area of the mold.
[0083] Considering the influence of the above factors on edge cracks in the cast billet, the formula for calculating the edge crack index is established as follows:
[0084]
[0085] In the formula: C: edge crack index;
[0086] X%: a percentage of online SEN export-side flow stocks;
[0087] Y%: Percentage of backflow at the lower edge of line b;
[0088] L: SEN outlet molten steel flow rate;
[0089] S: Cross-sectional area of the top opening of the crystallizer;
[0090] For a symmetrical double-outlet SEN, the continuous casting speed V is given by V = L / (ρ·S). Treating the steel density ρ as a constant, the edge crack index formula can be written as:
[0091] C = X%·Y%·V
[0092] In the two formulas above, the larger the X% value, the higher the temperature at the edge of the billet; the larger the Y% value, the slower the cooling rate of the billet shell at the edge; and the larger the L value, the higher the temperature of the molten steel reaching the edge, and the slower the cooling rate. These three values are directly proportional to the probability of edge cracks. Conversely, the smaller the S value, the weaker the cooling of the molten steel, the higher the temperature at the edge of the billet, and the more likely edge cracks will occur.
[0093] The larger the obtained edge crack index C value, the higher the temperature at the edge of the billet, the slower the cooling rate, and the greater the possibility of edge crack defects in the billet shell. This provides a specific and clearly evaluative quantitative index.
[0094] S4. Evaluation of Quantitative Index Values
[0095] By substituting the flow field quantification parameter values under various relevant process conditions or equipment structures into the calculation formula obtained in S3, the quantification index value for this defect under that condition can be obtained. The index values calculated under each condition are then analyzed and studied.
[0096] In this embodiment, the specific evaluation is as follows: at a certain SEN immersion depth, different continuous casting speeds and electromagnetic braking current values are substituted into the molten steel flow field analysis model to obtain the flow field quantitative parameter values, and the edge crack index C (e.g., ...) is calculated. Figure 3 As shown in the figure, the edge crack index increases with increasing casting speed, increasing the likelihood of edge cracks in the billet. Therefore, it can be said that the higher the casting speed, the more likely edge cracks will occur. Increasing the electromagnetic braking current can reduce the edge crack index. Thus, increasing the electromagnetic braking current when increasing the casting speed can improve the occurrence of edge cracks in the billet. This achieves multi-parameter quantitative evaluation of the molten steel flow field regarding edge cracks in the billet.
[0097] Example 2:
[0098] Taking a high-speed thin slab production line as an example, this quantitative evaluation method is used to evaluate different process parameters to address the problem of subsurface inclusion defects in the cast slab. This optimizes the production process, reduces casting defects, and improves production efficiency.
[0099] S1. Establish a defect mechanism model for cast billets.
[0100] In actual production, peeling / crack defects mainly occur in the middle of the billet, i.e., the SEN (Self-Exposed) region. Based on previous research and analysis specific to this production line, the formation mechanism of subsurface inclusion defects in the billet can be summarized as follows: Analyzing the source of inclusions, if they fail to rise to the surface of the molten steel and be captured by the protective slag, they will enter the interior of the billet, forming inclusions. Inclusions in the core of the billet are less likely to form defects, but if the inclusions are located close to the billet shell, they form subsurface inclusions, which can lead to peeling / crack defects during rolling.
[0101] S2. Establish a steel flow field analysis model.
[0102] S2.1 Establish a steel flow field analysis model and quantify the characteristics of the numerical simulation flow field.
[0103] This example uses Fluent simulation analysis software to establish a numerical simulation analysis model. For example... Figure 1 The diagram shows the flow field traces under the following process conditions: continuous casting speed of 5.2 m / min, electromagnetic braking current intensity of 175 A, and SEN immersion depth of 170 mm. Figure 4 The above simulation results are used for further analysis and calculation of subsurface inclusions in the cast billet. (1 / 4 symmetric diagram of molten steel surface velocity under these conditions.)
[0104] S2.2 Obtain the numerical model results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism.
[0105] Based on the molten steel flow field analysis model established in S2.1, the trajectory of inclusions forming defects is analyzed, such as... Figure 5 As shown: Inclusions enter the upper circulation of the flow field along the side flow ① and the upper backflow ② at the edge and begin to float. If they fail to float to the surface near ③, they will remain inside the billet in the region ④ near the SEN. In region ④, the molten steel flows downward, opposite to the upward direction of the inclusions, causing them to suspend and accumulate. At the same time, the billet shell is close and narrow in the outer region of SEN. Based on the factors that influence the molten steel flow field on the formation of this defect extracted from S1, inclusions in this region are very likely to approach the pasty area near the billet shell, forming subcutaneous inclusions. Therefore, a quantitative and evaluation model is established based on the source of molten steel inclusions in the crystallizer, the ease of floating, and the ease of suspension and enrichment near the billet shell.
[0106] Regarding the source of inclusions in molten steel, the main influencing factor is the proportion of upward backflow in the molten steel. The higher the proportion of upward backflow, the more subcutaneous inclusions can be formed.
[0107] The ease with which inclusions float in molten steel is primarily influenced by the surface velocity of the molten steel and the cross-sectional area of the crystallizer. A higher surface velocity makes it more difficult for inclusions to float to the surface. Conversely, a smaller crystallizer cross-sectional area also makes it more difficult for inclusions to float to the surface.
[0108] The main influencing factor on the ease with which inclusions in molten steel accumulate near the billet shell is the upper circulation velocity. The higher the upper circulation velocity, the easier it is for suspended inclusions to accumulate near the SEN.
[0109] Therefore, it is necessary to extract the proportion of circulating flow on the upper part of the stream and the flow velocity of the molten steel surface from the flow field calculation results.
[0110] The specific method for obtaining the values is the same as in Example 1. The proportion of SEN outlet side flow on line a and the proportion of backflow on the side of line b are obtained by the steel flow velocity distribution values on lines a and b, respectively.
[0111] S3. Establish the multi-parameter exponent value calculation formula.
[0112] Analysis of the flow field trace diagram obtained from S2 and the influencing factors obtained from S1 shows that the larger the proportion of upward backflow and the higher the upward backflow velocity, the more suspended and enriched inclusions are formed near SEN. The higher the liquid surface velocity and the smaller the cross-sectional area of the crystallizer, the more difficult it is for inclusions to float and be adsorbed by the protective slag. Therefore, the probability of forming subsurface inclusions in the cast billet is directly proportional to the proportion of sideflow and upward backflow, directly proportional to the liquid surface velocity, and inversely proportional to the cross-sectional area of the crystallizer.
[0113] The formula for calculating the subsurface inclusion index of the cast billet is as follows:
[0114]
[0115] In the formula: F: subcutaneous inclusion index;
[0116] X%: a percentage of online SEN export-side flow stocks;
[0117] Z%: Percentage of backflow along the edge of line b;
[0118] V: Maximum flow velocity at the surface of molten steel;
[0119] S: Cross-sectional area of the top opening of the crystallizer.
[0120] In the above formula, the product of X% and Z% is the proportion of the upper circulation. The larger the values of X% and Z%, the easier it is for inclusions to accumulate in the molten steel, and the greater the possibility of subcutaneous inclusions. V is used to characterize the surface velocity and upper circulation velocity of the molten steel. The larger this value, the easier it is for inclusions to accumulate in the molten steel. Conversely, the smaller the value of S, the easier it is for inclusions to accumulate in the molten steel, and the greater the possibility of subcutaneous inclusions.
[0121] The obtained subcutaneous inclusion index F is a specific quantitative index with clear evaluative significance: the larger the value, the easier it is for inclusions in the molten steel to form suspensions and enrich near SEN, and the greater the possibility of subcutaneous inclusion defects in the billet.
[0122] S4. Evaluation of Quantitative Index Values
[0123] By substituting the flow field quantification parameter values under various relevant process conditions or equipment structures into the calculation formula obtained in S3, the quantification index value for this defect under that condition can be obtained. The index values calculated under each condition are then analyzed and studied.
[0124] In this embodiment, the specific evaluation is as follows: at a certain SEN immersion depth, the subcutaneous inclusion index F under different continuous casting speeds and electromagnetic braking current values is as follows: Figure 6 As shown in the figure, the subsurface inclusion index increases with increasing casting speed, increasing the likelihood of subsurface inclusion defects in the billet. Therefore, it can be said that the higher the casting speed, the more likely subsurface inclusion defects will occur in the billet. Higher electromagnetic braking current values also increase the subsurface inclusion index. Therefore, when the casting speed is increased to 5.5 m / min, the electromagnetic braking current value should not be too high, but the impact of the current value is relatively small when the casting speed reaches 5.8 m / min. This study achieves multi-parameter quantitative evaluation of the molten steel flow field regarding subsurface inclusions in the billet.
[0125] In addition to quantifying and evaluating process condition parameters, the method of this invention can also provide guidance for equipment structure optimization through exponential values.
[0126] Example 3
[0127] Taking a high-speed thin slab production line as an example, this quantitative evaluation method is used to evaluate different SEN structures to address the problem of edge crack defects in slabs. This evaluation guides the design of SEN structures and develops SEN products that are more conducive to reducing edge crack defects in slabs, thereby improving slab quality and production efficiency.
[0128] S1. Establish a defect mechanism model for the cast billet (this step is the same as in Example 1).
[0129] S1.1 Determine the cause and mechanism of the formation of a certain defect in a cast billet that needs to be studied.
[0130] S1.2 clarifies the influencing factors of the molten steel flow field on the cause of this defect among the above causes.
[0131] S2. Establish a steel flow field analysis model.
[0132] S2.1 Establish a steel flow field analysis model and obtain the flow field numerical simulation analysis results under different conditions.
[0133] To address the factors caused by the molten steel flow field within the crystallizer as identified in S1.1, numerical simulation methods were employed to establish analytical models of the molten steel flow field under different SEN structures, which were then used to extract quantitative data.
[0134] In this embodiment, there are three SEN outlet cross-sectional dimensions (other dimensional parameters are the same) as follows: Figures 7-8 As shown:
[0135] Option A: w = 400mm, t = 70mm;
[0136] Option B: w = 475 mm, t = 70 mm;
[0137] Option C: w = 475 mm, t = 80 mm;
[0138] Where w is the width of the bottom opening of the SEN; t is the thickness of the bottom opening of the SEN.
[0139] Similar to Example 1, in the specific process of this example, Fluent simulation analysis software is used to establish a numerical simulation analysis model, and then the above three SEN structure schemes and different electromagnetic braking current intensities are simulated and analyzed respectively.
[0140] S2.2 Quantify the characteristics of the numerical simulation flow field, obtain the numerical simulation results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism. (This step is the same as in Example 1)
[0141] S3. Establish the multi-parameter index value calculation formula (this step is the same as in Example 1).
[0142] The formula for calculating the edge crack index is as follows:
[0143]
[0144] S4. Evaluation of Quantitative Index Values
[0145] By substituting the flow field quantification parameter values of the three SEN structural schemes and different electromagnetic braking current intensities into the calculation formula obtained in S3, the quantification index value for this defect under this condition can be obtained. The index values calculated under each condition are then analyzed and studied.
[0146] In this embodiment, the specific evaluation is as follows: Under a certain pulling speed and SEN immersion depth, different SEN structures and electromagnetic braking current values are substituted into the molten steel flow field analysis model to obtain the flow field quantitative parameter values, and the edge crack index C (e.g., ...) is calculated. Figure 9(As shown in the figure). It can be seen from the figure that increasing the SEN outlet cross-sectional size can significantly reduce the edge crack index value. Increasing the electromagnetic braking current value will further reduce it. Therefore, regarding the SEN structure, increasing the SEN outlet cross-sectional size can improve the occurrence of edge crack defects in the billet. This achieves a multi-parameter quantitative evaluation of the molten steel flow field regarding edge cracks in the billet. If edge crack defects in the billet are the main problem affecting billet quality and production efficiency during the production process of this line, increasing the SEN outlet cross-sectional size can be an optimization direction for the SEN structure dimensions. This achieves a quantitative evaluation of the SEN structure dimensions regarding edge cracks in the billet, and provides guidance for SEN structure design. In this embodiment, only three sets of dimensional parameters are used to illustrate the method process. In actual research, the influence of other process parameters or limitations such as equipment space need to be considered, and finally, multi-parameter cross-verification should be performed.
[0147] Similarly, this quantitative evaluation method is used to evaluate different copper plate shapes to guide copper plate shape design; and to evaluate different electromagnetic brake core positions to guide the structural design of electromagnetic brake equipment.
[0148] The quantitative index obtained by the method in this application is used for parameter evaluation and production guidance. The conclusions are consistent with the results in production practice. More importantly, this quantitative evaluation method has achieved theoretical proof of these conclusions.
[0149] The above embodiments are merely for specific description; other comparative analyses under various conditions are not listed here. Furthermore, the defect formation mechanisms vary depending on the production line. The calculation formulas in the specific embodiments of this application are only applicable to high-speed thin slab production lines; other production lines can be analyzed and obtained by referring to the method of this application.
[0150] It should be noted that the specific embodiments of the present invention have been described in detail. For those skilled in the art, various obvious changes made to it without departing from the spirit and scope of the present invention are within the protection scope of the present invention.
Claims
1. A mechanism model-based crystallizer molten steel flow field multi-parameter quantitative evaluation method, characterized in that: include: S1. Establish a defect mechanism model for cast billets: S1.1 Determine the cause and mechanism of a specific defect in a cast billet that needs to be studied; the defect in the cast billet is a subsurface inclusion defect. S1.2 Clarify the influencing factors of the molten steel flow field on the cause of this defect among the above causes; S2. Establish a steel flow field analysis model: S2.1 Numerical simulation methods are used to establish analytical models of molten steel flow field under different process conditions or equipment structures; S2.2 Quantify the characteristics of the numerical simulation flow field, obtain the numerical simulation results of the molten steel flow field under the required conditions, and extract the flow field parameters related to the defect formation mechanism; the specific method for parameter extraction is as follows: (1) Point P is the point where the molten steel reaches the edge of the crystallizer after flowing out of SEN and the flow velocity is the lowest. The value of D is the distance from point P to the liquid surface. (2) Line a is located 0.2m above point P, that is, D-0.2 is taken as the ordinate of line a. The distribution of molten steel velocity at line a is used to describe the circulation distribution in the flow field. (3) Line b is located 0.2m below point P, that is, D+0.2 is taken as the vertical coordinate of line b. The steel velocity distribution at line b is used to describe the circulation distribution under the flow field. (4) Obtain the flow velocity distribution values of molten steel on lines a and b, respectively, as well as the flow ratio of the flow towards the edge and the reverse flow ratio of the flow at the edge. S3. Establish a formula for calculating the parameter index value: Establish a formula for calculating the multi-parameter index value that can characterize the trend of this defect formation. Specifically: Establish the subsurface inclusion index F of the cast billet, and calculate the formula as follows: , Where: F: subcutaneous inclusion index; X%: percentage of SEN outlet flow on line a; Z%: percentage of backflow on the edge of line b; V: maximum flow velocity at the molten steel surface; S: Cross-sectional area of the top opening of the crystallizer; S4. Evaluation of Quantitative Index Value: Substitute the flow field quantitative parameter values under various relevant process conditions or equipment structures into the calculation formula obtained in S3 to obtain the quantitative index value of this defect under that condition.
2. The method according to claim 1, wherein the method is characterized by: The quantitative index value obtained in S4 is used to compare and analyze the advantages and disadvantages of different process conditions or equipment structures for a certain billet defect, and to analyze, study and optimize it.