A composite membrane material and its preparation method
By using a three-layer composite structure of polytetrafluoroethylene/carboxylated nanocellulose/polytetrafluoroethylene, the problems of insufficient heat resistance and electrolyte affinity of lithium-ion battery separator materials have been solved, resulting in higher battery safety and cycle performance.
Patent Information
- Application Number
- CN202311014782.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-09
AI Technical Summary
While existing lithium-ion battery separator materials improve heat resistance, they lack electrolyte affinity, which affects the battery's cycle performance and safety.
A three-layer composite structure of polytetrafluoroethylene/carboxylated nanocellulose/polytetrafluoroethylene is adopted, and the heat resistance and electrolyte affinity of the diaphragm are improved through biaxial stretching, hydrophilic modification and thermal composite preparation methods.
It significantly improves the heat resistance and electrolyte affinity of the separator, delays the occurrence of thermal runaway, and enhances the cycle performance and safety of the battery.
Smart Images

Figure CN116885384B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a composite separator material with high safety and high liquid retention rate and its preparation method. Background Technology
[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] Lithium-ion batteries, due to their high specific energy and long cycle performance, are considered a green new energy source and are currently widely used in electric vehicles and hybrid vehicles. Lithium-ion batteries mainly consist of positive and negative electrode materials, electrolyte, and separator. As one of the four main materials of lithium-ion batteries, the separator's rich microporous structure not only allows lithium ions to pass through but also isolates the positive and negative electrodes, preventing short circuits caused by contact between them. Therefore, the separator plays a crucial role not only in the rate performance and cycle performance of lithium batteries but also in battery safety.
[0004] Currently, commercially available separator materials mainly use polyethylene, polypropylene, and composite membranes formed by coating modified materials onto these two materials. Polyethylene and polypropylene materials are characterized by low price, chemical stability, and ease of processing. However, as the energy density of battery cell systems continues to increase, the safety requirements for various materials in battery systems are also increasing. While coating polyethylene and polypropylene separators with inorganic materials can improve their heat resistance, this cannot fundamentally change the limitations of the materials themselves and results in an overall thicker separator.
[0005] To improve the limitations of the heat resistance of the separator material itself, polytetrafluoroethylene (PTFE) can be used as the separator for lithium batteries. For example, patent CN102270756A designed a sandwich PTFE / polyethylene / PTFE structure lithium battery separator. However, due to the low surface energy of the PTFE layer and the lack of hydrophilic modification of the molecules, the separator has poor affinity with the electrolyte, which will seriously affect the cycle performance of the lithium battery.
[0006] Therefore, how to improve the heat resistance of polytetrafluoroethylene (PTFE) membranes while enhancing their electrolyte affinity is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the present invention aims to provide a composite membrane material and its preparation method. The composite membrane material of the present invention not only possesses superior heat resistance and dimensional stability compared to traditional polyolefin membranes, but also exhibits significantly improved affinity for electrolytes and electrolyte retention capacity, thereby enhancing the cycle performance and lifespan of the battery cell.
[0008] To achieve the above objectives, the technical solution of the present invention is as follows:
[0009] In a first aspect, the present invention provides a method for preparing a composite membrane material, the method comprising the following steps:
[0010] Polytetrafluoroethylene (PTFE) or a mixture thereof with additives is melted and then subjected to biaxial stretching to obtain a PTFE film. After hydrophilic modification and drying, a PTFE separator is obtained. Carboxylated nanocellulose slurry is coated on one side of the PTFE separator. After coating, it is thermally laminated with another PTFE separator to obtain a composite separator material with a three-layer composite structure of PTFE / carboxylated nanocellulose / PTFE.
[0011] Preferably, the mixture of polytetrafluoroethylene and additives is melted. The melting process includes the following steps:
[0012] 25wt%–70wt% polytetrafluoroethylene resin, 1wt%–5wt% inorganic filler, and 29wt%–70wt% paraffin oil are mixed and then fed into an extruder for melt blending, followed by extrusion through a die. The mixing temperature is 280℃–340℃, and the stirring speed is 90–120 rpm. The above mixing temperature is a general temperature for the entire process from melting to extrusion in the extruder; the melting and extrusion temperatures may be the same or different.
[0013] More preferably, the inorganic filler is one or more of alumina, boehmite, and nano-silica, and the particle size of the inorganic filler is 20-30 nm. The addition of the above-mentioned proportion of inorganic filler in this invention can appropriately reduce the crystallinity of polytetrafluoroethylene (PTFE), increase the proportion of amorphous regions, and improve ion permeability. Furthermore, the addition of the inorganic filler increases the degree of PTFE chain entanglement, weakening the molecular chain mobility, which is beneficial for improving tensile strength and elongation at break.
[0014] More preferably, the viscosity-average molecular weight of the polytetrafluoroethylene resin is 900,000 to 3,000,000.
[0015] Preferably, the biaxial stretching method includes the following steps:
[0016] Polytetrafluoroethylene (PTFE) or its mixture with additives is melted, biaxially stretched, extracted, biaxially stretched a second time, and shaped to obtain a PTFE film.
[0017] More preferably, the biaxial stretching temperature is 180℃~220℃, and the stretching ratio is 6~10 times. The biaxial stretching can improve the stretching uniformity of the diaphragm.
[0018] More preferably, the extraction is performed at room temperature; even more preferably, the product is dried after extraction at a temperature of 30–50°C.
[0019] More preferably, the second biaxial stretching and shaping is performed at a stretching temperature of 180℃~220℃, a stretching ratio of 5~10 times, and a shaping temperature of 120~150℃.
[0020] Preferably, the hydrophilic modification includes the following steps:
[0021] The shaped material is immersed in a solvent containing 1 wt% to 5 wt% modifier for 4 to 8 minutes for modification, followed by drying. Tetrafluoroethylene (TEF) exhibits hydrophobicity and oleophobicity due to its low surface tension (18.5 dyn / em) and low surface energy. This property does not meet the requirement of electrolyte affinity for the diaphragm, thus hydrophilic modification is necessary.
[0022] More preferably, the modifier includes polyvinyl acetate (PVAc) or a vinyl acetate-maleic anhydride copolymer. The polyvinyl acetate modifier can completely wet the PTFE membrane, and the PVAc molecular chain segments fully penetrate into the PTFE "fiber-node" network structure and attach to the PTFE fibrils, introducing hydroxyl groups onto the PTFE membrane surface. These hydroxyl groups are highly polar and exhibit hydrophilicity; therefore, this modification step is a hydrophilic modification. Due to the introduction of hydroxyl groups, they have a greater affinity for esters in the electrolyte, further reducing the contact angle of carbonate solvents with inherently low surface tension on the electrode and membrane surfaces. This reduction in membrane surface contact angle improves electrolyte wettability.
[0023] More preferably, the solvent includes silane coupling agent KH550, silane coupling agent KH560, or polyvinyl alcohol.
[0024] Preferably, the carboxylated nanocellulose slurry is composed of 20%–39% carboxylated nanocellulose, 0.2%–1% polyacrylamide, 0.2%–1% polyvinyl butyral, and 60%–79% pure water by mass percentage.
[0025] Preferably, the thermal bonding temperature is 100℃~120℃.
[0026] In a second aspect, the present invention provides a composite membrane material prepared by the above-described preparation method.
[0027] The present invention does not limit the thickness of each layer of the composite membrane material, as long as it is a three-layer structure of polytetrafluoroethylene / carboxylated nanocellulose / polytetrafluoroethylene. For example, the thickness of the polytetrafluoroethylene layer: the carboxylated nanocellulose coating: the polytetrafluoroethylene layer can be 1:1:1, or 2:1:2, or 3:1:3.
[0028] Compared with the prior art, the present invention has the following advantages:
[0029] In this invention, the polytetrafluoroethylene (PTFE) / carboxylated nanocellulose / PTFE three-layer structure utilizes the stable structure and high melting point of PTFE, resulting in significantly improved heat resistance compared to traditional polyethylene and polypropylene separators. Furthermore, the carboxylated nanocellulose coating between the PTFE layers has a lower melting point than PTFE. During the self-heating stage of thermal runaway in the battery cell, it melts and closes the pores, while the outer PTFE continues to provide mechanical support and physical isolation, delaying the onset of thermal runaway and improving the overall safety performance of the separator. In addition, the carboxylated nanocellulose exhibits stronger affinity for PTFE, better interfacial bonding between layers, and stronger affinity for the electrolyte, improving the separator's electrolyte retention rate and further enhancing battery cycle life. Moreover, its unique fibrous morphology results in larger interparticle spacing between the carboxylated nanocellulose particles compared to other materials, leading to improved Li... + It has better permeability and is more conducive to battery rate performance. Through coating and hydrophilic modification of polytetrafluoroethylene, the overall performance of the separator is safer and has a higher liquid retention rate. Attached Figure Description
[0030] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0031] Figure 1 This is a schematic diagram of the structure of the polytetrafluoroethylene / carboxylated nanocellulose / polytetrafluoroethylene composite membrane material of the present invention;
[0032] Figure 2 This is a SEM image of the polytetrafluoroethylene layer in Example 1 of the present invention;
[0033] Figure 3 The ionic conductivity of the membrane materials obtained in the embodiments and comparative examples of this invention;
[0034] Figure 4 The AC impedance of the diaphragm material obtained in the embodiments and comparative examples of the present invention is shown. Detailed Implementation
[0035] To improve the heat resistance of lithium-ion battery separators under high-temperature conditions and the affinity of polytetrafluoroethylene (PTFE) separators for electrolytes, this invention provides a composite separator material and its preparation method.
[0036] A first typical embodiment of the present invention provides a method for preparing a composite membrane material, the method comprising the following steps:
[0037] After melting polytetrafluoroethylene (PTFE), it is subjected to biaxial stretching, extraction, a second biaxial stretching and shaping, hydrophilic modification, and drying to obtain a PTFE membrane. Carboxylated nanocellulose slurry is coated on one side of the PTFE membrane. After coating, it is thermally composited with another PTFE membrane to obtain a composite membrane material with a three-layer composite structure of PTFE / carboxylated nanocellulose / PTFE.
[0038] Thanks to the superior structure and chemical stability of polytetrafluoroethylene (PTFE), this type of separator exhibits significantly improved mechanical properties and heat resistance compared to traditional separator materials. By introducing carboxylated cellulose nanoparticles with electrolyte affinity into the PTFE layer, the excellent physicochemical properties of carboxylated cellulose nanoparticles, combined with surface modification, greatly enhance the electrolyte affinity and electrolyte retention capacity of PTFE. The physicochemical properties of carboxylated cellulose nanoparticles differ significantly from those of traditional cellulose nanoparticles, primarily in the following aspects:
[0039] (1) Morphology and structure: Carboxylated nanocellulose typically has a diameter of 10-20 nanometers and a length of several micrometers to tens of micrometers, exhibiting a fibrous morphology.
[0040] (2) Water solubility: Carboxylated nanocellulose has good water solubility and dispersibility, and can form a colloidal solution in water, which can be applied to the preparation of nanocomposite materials;
[0041] (3) Surface charge properties: Carboxylated nanocellulose has a negative charge on its surface, which can interact with positively charged polymers, increase the interfacial adhesion of polymers, and thus improve the mechanical properties of composite materials.
[0042] (4) Melting point: Carboxylated nanocellulose has a low melting point, usually between 150-200℃.
[0043] The sandwich-structured composite separator of the present invention has better heat resistance and dimensional stability than traditional polyolefin separators, and also has a higher liquid retention rate, which can improve the cycle performance and service life of the battery cell.
[0044] In some embodiments of this implementation, the melting process includes the following steps:
[0045] 25wt%–70wt% of polytetrafluoroethylene resin, 1wt%–5wt% of inorganic filler, and 29wt%–70wt% of paraffin oil are mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature is 280℃–340℃, and the stirring speed is 90–120 rpm.
[0046] The inorganic filler is one or more of alumina, boehmite, and nano-silica.
[0047] The viscosity-average molecular weight of the polytetrafluoroethylene resin is 900,000 to 3,000,000.
[0048] In some embodiments of this implementation, the stretching temperature of the biaxial stretching is 180℃~220℃, and the stretching ratio is 6~10 times.
[0049] In some embodiments of this implementation, the extraction is performed at room temperature; preferably, the material is dried after extraction at a temperature of 30–50°C.
[0050] In some embodiments of this implementation, the second biaxial stretching and shaping is performed at a stretching temperature of 180°C to 220°C, a stretching ratio of 5 to 10 times, and a shaping temperature of 120°C to 150°C.
[0051] In some embodiments of this implementation, the hydrophilic modification includes the following steps:
[0052] The shaped material is immersed in a solvent containing 1 wt% to 5 wt% modifier for immersion modification for 4 to 8 minutes, and then dried after immersion.
[0053] The modifiers include, but are not limited to, polyvinyl acetate and vinyl acetate-maleic anhydride copolymer.
[0054] The solvents include, but are not limited to, silane coupling agent KH550, silane coupling agent KH560, and polyvinyl alcohol.
[0055] In some embodiments of this implementation, the carboxylated nanocellulose slurry, by mass percentage, consists of 20%–39% carboxylated nanocellulose, 0.2%–1% polyacrylamide, 0.2%–1% polyvinyl butyral, and 60%–79% pure water.
[0056] In some embodiments of this implementation, the thermal bonding temperature is 100℃~120℃.
[0057] Another typical embodiment of the present invention provides a composite membrane material, which is prepared by the above-described preparation method.
[0058] In some embodiments of this implementation, the thickness of the polytetrafluoroethylene layer: the carboxylated nanocellulose coating: the thickness of the polytetrafluoroethylene layer = 2:1:2.
[0059] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0060] Scanning electron microscope (SEM) images: The surface morphology of the material was characterized using a scanning electron microscope (SEM). The SEM used was a Zeiss Sigma 300, and the testing conditions were: drying, gold plating, and a voltage of 15 kV.
[0061] Ionic conductivity: The ionic conductivity of the membrane material is calculated by obtaining the membrane internal resistance Rb from the AC impedance spectroscopy. The device used is a VersaSTAT200. The detection conditions are as follows: the membrane is sandwiched between two 16mm stainless steel sheets, and an appropriate amount of electrolyte is added to assemble a CR2025 button cell. The scanning frequency is 1... -1 Hz~1×10 6 With an AC amplitude of 10mV and a frequency of Hz, the AC impedance spectrum of the battery can be obtained. The value at the intersection of the graph and the horizontal axis represents the resistance Rb of the separator, where S is the area of the stainless steel sheet. The resistance can be calculated using the formula: σ = d / (R... b *S), where d is the diaphragm thickness.
[0062] Example 1
[0063] A method for preparing a composite membrane material includes the following steps:
[0064] (1) 25 wt% polytetrafluoroethylene resin, 5 wt% alumina (Al2O3), and 70 wt% paraffin oil were mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature T = 320℃ and the stirring speed n = 90 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 900,000.
[0065] (2) The sheet from step (1) is subjected to biaxial stretching at a stretching temperature of 210℃ and a stretching ratio of 6 times.
[0066] (3) The material obtained in step (2) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0067] (4) The material obtained in step (3) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 8 times, and a shaping temperature of 120°C.
[0068] (5) The material obtained in step (4) is immersed in a solvent containing 2 wt% modifier for modification for 5 minutes, and then dried after immersion. The modifier is vinyl acetate-maleic anhydride copolymer. The solvent is polyvinyl alcohol (PVC).
[0069] (6) Prepare the coating slurry: 30% carboxylated nanocellulose, 0.2% polyacrylamide, 0.2% polyvinyl butyral, and 69.6% pure water (by mass).
[0070] (7) The slurry obtained in step (6) is coated onto the sheet obtained in step (5) using a gravure roller and then dried.
[0071] (8) Perform thermal bonding between the material obtained in step (7) and the material obtained in step (5). The bonding temperature is 110℃.
[0072] (9) Roll up the material obtained in step (8).
[0073] This invention designs a polytetrafluoroethylene / carboxylated nanocellulose / polytetrafluoroethylene three-layer composite structure, through... Figure 1 The electron micrographs reveal abundant porous structures within the polytetrafluoroethylene layer.
[0074] Example 2
[0075] A method for preparing a composite membrane material includes the following steps:
[0076] (1) 20 wt% polytetrafluoroethylene resin, 1 wt% alumina (Al2O3), and 79 wt% paraffin oil were mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature T = 320℃ and the stirring speed n = 90 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 900,000.
[0077] (2) The sheet from step (1) is subjected to biaxial stretching at a stretching temperature of 210℃ and a stretching ratio of 6 times.
[0078] (3) The material obtained in step (2) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0079] (4) The material obtained in step (3) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 8 times, and a shaping temperature of 120°C.
[0080] (5) The material obtained in step (4) is immersed in a solvent containing 2 wt% modifier for modification for 5 minutes, and then dried after immersion. The modifier is vinyl acetate-maleic anhydride copolymer. The solvent is polyvinyl alcohol (PVC).
[0081] (6) Prepare the coating slurry: 30% carboxylated nanocellulose, 0.2% polyacrylamide, 0.2% polyvinyl butyral, and 69.6% pure water (by mass).
[0082] (7) The slurry obtained in step (6) is coated onto the sheet obtained in step (5) using a gravure roller and then dried.
[0083] (8) Perform thermal bonding between the material obtained in step (7) and the material obtained in step (5). The bonding temperature is 110℃.
[0084] (9) Roll up the material obtained in step (8).
[0085] Example 3
[0086] A method for preparing a composite membrane material includes the following steps:
[0087] (1) 25 wt% polytetrafluoroethylene resin, 5 wt% boehmite (γ-AlOOH), and 70 wt% paraffin oil were mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature T = 320℃ and the stirring speed n = 90 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 900,000.
[0088] (2) The sheet from step (1) is subjected to biaxial stretching at a stretching temperature of 210℃ and a stretching ratio of 6 times.
[0089] (3) The material obtained in step (2) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0090] (4) The material obtained in step (3) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 8 times, and a shaping temperature of 120°C.
[0091] (5) The material obtained in step (4) is immersed in a solvent containing 2 wt% modifier for modification for 5 minutes, and then dried after immersion. The modifier is vinyl acetate-maleic anhydride copolymer. The solvent is polyvinyl alcohol (PVC).
[0092] (6) Prepare the coating slurry: 30% carboxylated nanocellulose, 0.2% polyacrylamide, 0.2% polyvinyl butyral, and 69.6% pure water (by mass).
[0093] (7) The slurry obtained in step (6) is coated onto the sheet obtained in step (5) using a gravure roller and then dried.
[0094] (8) Perform thermal bonding between the material obtained in step (7) and the material obtained in step (5). The bonding temperature is 110℃.
[0095] (9) Roll up the material obtained in step (8).
[0096] Example 4
[0097] A method for preparing a composite membrane material includes the following steps:
[0098] (1) 25 wt% polytetrafluoroethylene resin, 5 wt% alumina (Al2O3), and 70 wt% paraffin oil were mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature T = 320℃ and the stirring speed n = 90 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 3,000,000.
[0099] (2) The sheet from step (1) is subjected to biaxial stretching at a stretching temperature of 210℃ and a stretching ratio of 6 times.
[0100] (3) The material obtained in step (2) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0101] (4) The material obtained in step (3) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 8 times, and a shaping temperature of 120°C.
[0102] (5) The material obtained in step (4) is immersed in a solvent containing 2 wt% modifier for modification for 5 minutes, and then dried after immersion. The modifier is vinyl acetate-maleic anhydride copolymer. The solvent is polyvinyl alcohol (PVC).
[0103] (6) Prepare the coating slurry: 30% carboxylated nanocellulose, 0.2% polyacrylamide, 0.2% polyvinyl butyral, and 69.6% pure water (by mass).
[0104] (7) The slurry obtained in step (6) is coated onto the sheet obtained in step (5) using a gravure roller and then dried.
[0105] (8) Perform thermal bonding between the material obtained in step (7) and the material obtained in step (5). The bonding temperature is 110℃.
[0106] (9) Roll up the material obtained in step (8).
[0107] Comparative Example 1
[0108] (1) 25 wt% polytetrafluoroethylene resin, 5 wt% alumina (Al2O3), and 70 wt% paraffin oil were mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature T = 320℃ and the stirring speed n = 90 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 900,000.
[0109] (2) The sheet obtained in step (1) is subjected to biaxial stretching at a stretching temperature of 210℃ and a stretching ratio of 6 times.
[0110] (3) The material obtained in step (2) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0111] (4) The material obtained in step (3) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 8 times, and a shaping temperature of 120°C.
[0112] (5) The material obtained in step (4) is immersed in a solvent containing 2 wt% modifier for modification for 5 minutes, and then dried after immersion. The modifier is vinyl acetate-maleic anhydride copolymer. The solvent is polyvinyl alcohol (PVC).
[0113] (6) Prepare the coating slurry: 30% nano SiO2, 0.2% polyacrylamide, 0.2% polyvinyl butyral, 69.6% pure water (mass percentage).
[0114] (7) The slurry obtained in step (6) is coated onto the sheet obtained in step (5) using a gravure roller and then dried.
[0115] (8) Perform thermal bonding between the material obtained in step (7) and the material obtained in step (5). The bonding temperature is 110℃.
[0116] (9) Roll up the material obtained in step (8).
[0117] Comparative Example 2
[0118] A method for preparing a polytetrafluoroethylene / polyethylene / polytetrafluoroethylene membrane material includes the following steps:
[0119] (1) 40 wt% polytetrafluoroethylene resin and 60 wt% paraffin oil were mixed and then fed into an extruder for melt blending. The resulting melt was called melt A. The mixing temperature was T = 340℃ and the stirring speed was n = 100 rpm. The viscosity-average molecular weight of the polytetrafluoroethylene resin was 1,650,000.
[0120] (2) 30 wt% polyethylene resin and 70 wt% paraffin oil were mixed and then fed into an extruder for melt blending. The resulting melt was melt B. The mixing temperature was T = 190℃, and the stirring speed was n = 75 rpm. The viscosity-average molecular weight of the polyethylene resin was 1,200,000.
[0121] (3) Melt A and melt B are extruded through a three-channel co-extrusion die to form an A / B / A structure sheet. The composite temperature is 190℃.
[0122] (4) The sheet obtained in step (3) is subjected to biaxial stretching at a stretching temperature of 210°C and a stretching ratio of 8 times.
[0123] (5) The material obtained in step (4) is extracted by immersing it in dichloromethane and then dried. The extraction temperature is room temperature and the drying temperature is 40°C.
[0124] (6) The material obtained in step (5) is immersed in a silane coupling agent KH550 containing 2 wt% polyvinyl acetate for modification. The immersion time is 5 min, and the material is dried after immersion.
[0125] (7) Dry the material obtained in step (6).
[0126] (8) The material obtained in step (7) is subjected to biaxial stretching and shaping at a stretching temperature of 210°C, a stretching ratio of 10 times, and a shaping temperature of 120°C.
[0127] (9) Roll up the material obtained in step (8).
[0128] Performance testing:
[0129] The mechanical properties, heat resistance, and liquid retention rate of the diaphragm materials obtained in the examples and comparative examples were tested. The air permeability was tested according to GB / T 36363-2018; the tensile strength was tested according to GB / T1040.3-2006; the needle penetration strength was tested according to GB / T 10004-2008; the heat shrinkage MD / TD was tested according to GB / T 36363-2018; and the liquid retention rate was tested by immersing the diaphragm in the electrolyte and calculating the ratio of the mass difference of the diaphragm before and after liquid absorption to the mass of the substrate diaphragm. The test results are shown in Table 1.
[0130] Table 1. Performance comparison of the membrane materials obtained in the examples and comparative examples.
[0131]
[0132]
[0133] As shown in Table 1, the polytetrafluoroethylene / carboxylated nanocellulose / polytetrafluoroethylene composite membrane of the examples is superior to the nano-SiO2 filled membrane (Comparative Example 1) and the PE composite membrane (Comparative Example 2) in terms of air permeability and heat resistance, and the improvement is more significant. In addition, due to the abundant hydroxyl and carboxyl groups on the surface of carboxylated nanocellulose, the membrane has a higher affinity for electrolyte, resulting in a higher electrolyte retention rate.
[0134] The electrical properties of the diaphragm materials obtained in the examples and comparative examples were tested, wherein:
[0135] The method for testing ionic conductivity (σ) is as follows: the ionic conductivity of the membrane material is calculated by obtaining the membrane internal resistance Rb from the AC impedance spectrum. The equipment used is a VersaSTAT200, and the testing conditions are: the membrane is sandwiched between two 16mm stainless steel sheets, and an appropriate amount of electrolyte is added, assembling a CR2025 button cell. The scanning frequency is 1Hz~1×10⁻⁶. 6With an AC frequency of Hz and an AC amplitude of 10mV, the AC impedance spectrum of the battery can be obtained. The value at the intersection of the graph and the horizontal axis is the resistance R of the separator. b S is the area of the stainless steel sheet. The calculation formula is: σ=d / (R) b *S), where d is the diaphragm thickness.
[0136] The method for testing AC impedance is as follows: CR2025 half-cells containing samples with different separators are left to stand for 24 hours, then subjected to a constant current charge-discharge cycle at a current density of 0.1C. The results are then obtained using an electrochemical workstation with a scan frequency set to 0.01Hz~1×10⁻⁶. 5 With an AC amplitude of 10mV and a frequency of Hz, the AC impedance spectra of lithium-ion batteries containing different separator samples can be obtained, and the AC impedance can be obtained by reading the horizontal axis of the spectrum.
[0137] The test results are shown in Table 2.
[0138] Table 2 Comparison of ionic conductivity and AC impedance parameters of the membrane materials obtained in the examples and comparative examples.
[0139] parameter Example 1 Comparative Example 1 Comparative Example 2 <![CDATA[Ionic conductivity R b (Ω)]]> 3.41 2.9 1.15 <![CDATA[AC impedance R ct (Ω)]]> 34.3 31.6 21.87
[0140] As shown in Table 2, a comparison of the ionic conductivity and AC impedance of Example 1 with Comparative Examples 1 and 2 reveals that, due to the negative charge on the surface of carboxylated nanocellulose, it can interact with positively charged polymers, increasing the interfacial adhesion of the polymers. Furthermore, carboxylated nanocellulose exhibits a higher affinity for the electrolyte, and its unique fibrous morphology is more conducive to Li… + The carboxylated nanocellulose coating, after thermal lamination, exhibits superior compatibility with polytetrafluoroethylene (PTFE) compared to inorganic nano-SiO2 and PE particles, showing lower interfacial blocking effects and thus lower overall internal resistance. Nano-SiO2, due to its spherical morphology and high packing density, has smaller interparticle spacing than carboxylated nanocellulose, resulting in higher overall impedance. The PTFE / PE / PTFE three-layer composite membrane also exhibits higher overall impedance due to interlayer interfacial impedance effects and discontinuities.
[0141] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a composite membrane material, characterized in that, The preparation method includes the following steps: Polytetrafluoroethylene (PTFE) or a mixture thereof with additives is melted and then subjected to biaxial stretching to obtain a PTFE film. After hydrophilic modification and drying, a PTFE membrane is obtained. Carboxylated nanocellulose slurry is coated on one side of the PTFE membrane. After coating, it is thermally laminated with another PTFE membrane to obtain a composite membrane material with a three-layer composite structure of PTFE / carboxylated nanocellulose / PTFE.
2. The preparation method according to claim 1, characterized in that, The mixture of polytetrafluoroethylene and additives is melted; the melting process includes the following steps: 25wt%~70wt% of polytetrafluoroethylene resin, 1wt%~5wt% of inorganic filler, and 29wt%~70wt% of paraffin oil are mixed and fed into an extruder for melt blending, and then extruded through a die. The mixing temperature is 280℃~340℃ and the stirring speed is 90~120rpm.
3. The preparation method according to claim 2, characterized in that, The inorganic filler is one or more of alumina, boehmite, and nano-silica; the particle size of the inorganic filler is 20~30 nm. Alternatively, the viscosity-average molecular weight of the polytetrafluoroethylene resin is 900,000 to 3,000,000.
4. The preparation method according to claim 1, characterized in that, The biaxial stretching method includes the following steps: Polytetrafluoroethylene (PTFE) or a mixture thereof with additives is melted, biaxially stretched, extracted, biaxially stretched a second time, and shaped to obtain a PTFE film.
5. The preparation method according to claim 4, characterized in that, The stretching temperature of the biaxial stretching is 180℃~220℃, and the stretching ratio is 6~10 times. Alternatively, the extraction is performed at room temperature; after extraction, the material is dried at a temperature of 30-50°C. Alternatively, the second biaxial stretching and shaping is performed at a stretching temperature of 180℃~220℃, a stretching ratio of 5~10 times, and a shaping temperature of 120~150℃.
6. The preparation method according to claim 1, characterized in that, The hydrophilic modification includes the following steps: The polytetrafluoroethylene film was immersed in a solvent containing 1 wt% to 5 wt% modifier for 4 to 8 minutes, and then dried after immersion.
7. The preparation method according to claim 6, characterized in that, The modifier includes polyvinyl acetate or vinyl acetate-maleic anhydride copolymer.
8. The preparation method according to claim 1, characterized in that, The carboxylated nanocellulose slurry, by mass percentage, consists of 20%~39% carboxylated nanocellulose, 0.2%~1% polyacrylamide, 0.2%~1% polyvinyl butyral, and 60%~79% pure water.
9. The preparation method according to claim 1, characterized in that, The thermal bonding process takes place at a temperature of 100℃~120℃.
10. A composite membrane material, characterized in that, It is prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
Composite separator for lithium-ion batteries
CN102270756A
Ceramic separation membrane, lithium ion battery, and preparation methods of ceramic separation membrane and lithium ion battery
CN107799702A
Micropore separation membrane and its manufacturing method of bidrectional tensile coating for lithium ion batteries
KR102331373B1