A lithium battery positive electrode material and preparation method thereof

By using the Humemrs method to prepare graphene oxide in the positive electrode material of lithium battery, combined with nickel acetate, polyether F127 and dopamine, a porous structure is formed, which solves the problem of insufficient circulation and rate performance of lithium batteries, and significantly improves lithium batteries specific capacity and cycle stability.

CN116895749BActive Publication Date: 2024-11-01智泰新能源(东台)有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310873609.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-17
Publication Date
2024-11-01
Estimated Expiration
2043-07-17

AI Technical Summary

Technical Problem

The existing lithium battery positive electrode materials have shortcomings in circulation and rate performance, making it difficult to improve energy storage efficiency.

Method used

Graphene oxide was prepared as a support by Humemrs method, and the polyether F127 and 1,3,5-trimethylbenzene templates were self-assembled to form a porous structure, combining dopamine and palladium catalysts to form a polyphenylaline structure , improve specific capacity and cycle stability.

Benefits of technology

It significantly improves the specific capacity and cycle stability of lithium batteries, promotes the transportation of electrolyte and oxygen, and enhances the formation and decomposition of discharge products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a lithium battery positive electrode material and a preparation method thereof, comprising the following steps: step S1, preparing a carrier; step S2, adding polyether and 1,3,5-trimethylbenzene into an ethanol aqueous solution, adding a Tris buffer, adding the carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, centrifuging for 5 minutes, collecting precipitation, and preparing a composite carrier; step S3, adding the composite carrier into a three-necked flask, adding o-xylene, then sequentially adding 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate, then dripping an o-xylene solution of tri-tert-butylphosphine, reflux reacting for 12 hours, and preparing the lithium battery positive electrode material; porous graphene is used as a carrier, and the special porous structure can promote the transportation of electrolyte and oxygen, is conducive to promoting the formation and decomposition of discharge products, and forms a multi-component composite positive electrode material, and the positive electrode material prepared by the method can give the lithium battery a higher specific capacity and cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a field, and in particular to a lithium battery positive electrode material and a preparation method thereof. Background Art

[0002] Lithium battery is a kind of battery that uses lithium metal or lithium alloy as positive / negative electrode material and non-aqueous electrolyte solution; the existing lithium battery positive electrode materials mainly include lithium iron phosphate, nickel cobalt manganese ternary, etc. The theoretical specific capacity of lithium iron phosphate is about 170mAh / g. Studies have found that the theoretical specific capacity of lithium iron borate is about 220mAh / g, which is greater than the theoretical specific capacity of lithium iron phosphate. This material can be used as an alternative to lithium iron phosphate. It has higher specific capacity, better conductivity, and extremely small volume change rate; lithium iron borate, as a new lithium-ion nano positive electrode material, is gaining more and more attention.

[0003] As a conductive material, graphene can well promote the insertion and extraction of ions, thus showing good positive electrode material properties. Experimental results show that in lithium-ion batteries, graphene materials have better energy storage than traditional carbon negative electrode materials, greatly improving the energy storage efficiency of lithium-ion batteries. However, how to improve the cycle performance and rate performance is still a technical problem that needs to be solved urgently. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a lithium battery positive electrode material and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a positive electrode material for a lithium battery comprises the following steps:

[0007] Step S1, adding graphene oxide prepared by the Humems method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% by mass nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it until solidification after the ultrasonication to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 5-10°C / min, calcining it for 1 hour, then cooling it to room temperature to obtain a crude carrier, then transferring it to a 10% by mass hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier;

[0008] In step S1, graphene oxide is used as a matrix and nickel acetate is used as an etchant, followed by calcination. The nickel-based substance reacts with graphene at a high temperature, so that the carbon atoms on the surface of the graphene are oxidized into carbon oxide gas and then removed. The metal nickel is then removed by washing with hydrochloric acid to prepare a carrier with different pore structures. The special porous structure can promote the transportation of electrolyte and oxygen, and is conducive to promoting the formation and decomposition of discharge products.

[0009] Step S2, adding polyether (F127) and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution, then adding a Tris buffer solution with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier;

[0010] In step S2, polyether (F127) acts as a surfactant and pore expansion agent 1,3,5-trimethylbenzene to form a template, and then dopamine is self-assembled and polymerized on the template to form polydopamine, and can undergo π-π stacking with 1,3,5-trimethylbenzene to enter the interior of the template and finally exit the template, so as to form a porous polydopamine structure on the carrier surface, and the polydopamine is coated on the carrier surface. Through its own special porous structure, the influence of the coating structure on the carrier pores is reduced.

[0011] Step S3, adding the composite carrier into a three-necked flask, adding o-xylene, then adding 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purging under argon atmosphere and stirring at high speed for 15 minutes, then dropping a solution of tri-tert-butylphosphine in o-xylene, purging with argon for 10 minutes, heating to 160° C., and reflux reaction for 12 hours to obtain a positive electrode material for a lithium battery;

[0012] In step S3, 4-bromodiphenylamine is used as a monomer to carry out an aromatic amination reaction under the action of a palladium catalyst to prepare polyphenylaniline. The polytriphenylamine structure in the structure can improve the specific capacity and cycle stability of the lithium battery.

[0013] Furthermore: in step S1, the dosage ratio of graphene oxide, nickel acetate and deionized water is controlled to be 150-200 mg: 15-20 mg: 100 mL.

[0014] Furthermore, in step S2, the weight ratio of polyether (F127), 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine is controlled to be 200 mg: 200 mg: 20 mg: 100-150 mg: 50-60 mg.

[0015] Further: in step S3, the dosage ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 30-50 mg: 10.24-10.28 mg: 21 mg: 0.4-0.5 mg: 50 mL: 0.4 mmol.

[0016] Furthermore, the tri-tert-butylphosphine o-xylene solution in step S3 is prepared by mixing tri-tert-butylphosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL.

[0017] A lithium battery positive electrode material is prepared by the above preparation method.

[0018] Beneficial effects of the present invention:

[0019] The invention prepares a positive electrode material for a lithium battery. The porous graphene is used as a carrier. The special porous structure can promote the transportation of electrolyte and oxygen, and is beneficial to promoting the formation and decomposition of discharge products. Then, polyether (F127) is used as a surfactant and 1,3,5-trimethylbenzene as a pore expansion agent to form a template in coordination. Then, dopamine is self-assembled and polymerized on the template to form polydopamine, and can undergo π-π stacking with 1,3,5-trimethylbenzene to enter the interior of the template. Finally, the template is removed until a porous polydopamine structure is formed on the surface of the carrier. The polydopamine is coated on the surface of the carrier. The special porous structure of the polydopamine reduces the influence of the coating structure on the pores of the carrier. Finally, the polyphenylaniline synthesized is adhered by the adhesion characteristics of the polydopamine to form a multi-component composite positive electrode material. Therefore, the positive electrode material prepared by the method can give the lithium battery a higher specific capacity and cycle stability. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0021] A method for preparing a positive electrode material for a lithium battery comprises the following steps:

[0022] Step S1, adding the graphene oxide prepared by the Humemrs method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it until solidification after the ultrasonication to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 5°C / min, calcining it for 1 hour, then cooling it to room temperature to obtain a crude carrier, then transferring it to a 10% hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier, and controlling the amount ratio of graphene oxide, nickel acetate and deionized water to be 150mg:15mg:100mL;

[0023] Step S2, adding polyether (F127) and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution by volume, then adding Tris buffer with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier, and controlling the weight ratio of polyether (F127), 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine to be 200 mg: 200 mg: 20 mg: 100 mg: 50 mg;

[0024] Step S3, add the composite carrier to a three-necked flask, add o-xylene, then add 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purge under argon atmosphere and stir at high speed for 15 minutes, then dropwise add a solution of tri-tert-butylphosphine in o-xylene, purge with argon for 10 minutes, heat to 160°C, reflux for 12 hours, and obtain a positive electrode material for a lithium battery, wherein the amount ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 30 mg: 10.24 mg: 21 mg: 0.4 mg: 50 mL: 0.4 mmol.

[0025] The tri-tert-butyl phosphine o-xylene solution is prepared by mixing tri-tert-butyl phosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL. Example 2

[0026] A method for preparing a positive electrode material for a lithium battery comprises the following steps:

[0027] Step S1, adding the graphene oxide prepared by the Humems method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it after the ultrasonication until solidification, to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 10°C / min, calcining it for 1 hour, then cooling it to room temperature, to obtain a crude carrier, then transferring it to a 10% hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier, and controlling the amount ratio of graphene oxide, nickel acetate and deionized water to be 160mg:16mg:100mL;

[0028] Step S2, adding polyether (F127) and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution by volume, then adding Tris buffer with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier, and controlling the weight ratio of polyether (F127), 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine to be 200 mg: 200 mg: 20 mg: 120 mg: 52 mg;

[0029] Step S3, add the composite carrier to a three-necked flask, add o-xylene, then add 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purge under argon atmosphere and stir at high speed for 15 minutes, then dropwise add a solution of tri-tert-butylphosphine in o-xylene, purge with argon for 10 minutes, heat to 160°C, reflux for 12 hours, and obtain a positive electrode material for a lithium battery, wherein the amount ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 35 mg: 10.26 mg: 21 mg: 0.4 mg: 50 mL: 0.4 mmol.

[0030] The tri-tert-butyl phosphine o-xylene solution is prepared by mixing tri-tert-butyl phosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL. Example 3

[0031] A method for preparing a positive electrode material for a lithium battery comprises the following steps:

[0032] Step S1, adding the graphene oxide prepared by the Humemrs method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it after the ultrasonication until solidification, to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 5°C / min, calcining it at this temperature for 1 hour, then cooling it to room temperature, to obtain a crude carrier, then transferring it to a 10% hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier, and controlling the amount ratio of graphene oxide, nickel acetate and deionized water to be 180 mg: 18 mg: 100 mL;

[0033] Step S2, adding polyether (F127) and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution by volume, then adding Tris buffer with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier, and controlling the weight ratio of polyether (F127), 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine to be 200 mg: 200 mg: 20 mg: 140 mg: 58 mg;

[0034] Step S3, add the composite carrier to a three-necked flask, add o-xylene, then add 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purge under argon atmosphere and stir at high speed for 15 minutes, then dropwise add a solution of tri-tert-butylphosphine in o-xylene, purge with argon for 10 minutes, heat to 160°C, reflux for 12 hours, and obtain a positive electrode material for a lithium battery, wherein the amount ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 45 mg: 10.28 mg: 21 mg: 0.5 mg: 50 mL: 0.4 mmol.

[0035] The tri-tert-butyl phosphine o-xylene solution is prepared by mixing tri-tert-butyl phosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL. Example 4

[0036] A method for preparing a positive electrode material for a lithium battery comprises the following steps:

[0037] Step S1, adding the graphene oxide prepared by the Humemrs method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it after the ultrasonication until solidification, to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 10°C / min, calcining it for 1 hour, then cooling it to room temperature, to obtain a crude carrier, then transferring it to a 10% hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier, and controlling the amount ratio of graphene oxide, nickel acetate and deionized water to be 200 mg: 20 mg: 100 mL;

[0038] Step S2, adding polyether (F127) and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution by volume, then adding Tris buffer with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier, and controlling the weight ratio of polyether (F127), 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine to be 200 mg: 200 mg: 20 mg: 150 mg: 60 mg;

[0039] Step S3, add the composite carrier to a three-necked flask, add o-xylene, then add 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purge under argon atmosphere and stir at high speed for 15 minutes, then dropwise add a solution of tri-tert-butylphosphine in o-xylene, purge with argon for 10 minutes, heat to 160°C, reflux for 12 hours, and obtain a positive electrode material for a lithium battery, wherein the amount ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 50 mg: 10.28 mg: 21 mg: 0.5 mg: 50 mL: 0.4 mmol.

[0040] The tri-tert-butyl phosphine o-xylene solution is prepared by mixing tri-tert-butyl phosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL.

[0041] Comparative Example 1

[0042] Compared with Example 1, this comparative example uses graphene as the positive electrode material.

[0043] Comparative Example 2

[0044] This comparative example is a commercially available sulfur-carbon composite positive electrode material.

[0045] The positive electrode materials, acetylene black and polyethylene oxide prepared in Example 1-4 and Comparative Example 1-2 were uniformly coated on the current collector, dried at 22° C. for 20 h, and cut into 1×1 cm 2 The electrode was dried in a vacuum oven at 65°C for 10 h to obtain a positive electrode. The lithium sheet was used as the negative electrode, the separator was PVDF-HFP, and the electrolyte was LiPF6 / EC-DMC-EMC (1:1:1) with a molar concentration of 1 mol / L. The simulated battery was assembled in a glove box with an argon atmosphere, and the assembled battery samples were tested for charge and discharge performance at 25°C. The charge and discharge current density was 0.6 mA cm 2 , the test voltage range is 1.8-3.0V, the results are shown in Table 1 below:

[0046] Discharge capacity mAh / g Specific capacity mAh / g after 120 cycles Example 1 1478 1215 Example 2 1481 1220 Example 3 1480 1218 Example 4 1482 1223 Comparative Example 1 987 440 Comparative Example 2 1260 886

[0047] It can be seen from Table 1 above that the positive electrode materials prepared in Examples 1-4 of the present invention can improve the specific capacity and cycle stability of the battery.

[0048] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a positive electrode material for a lithium battery, characterized in that: The steps include: Step S1, adding graphene oxide prepared by the Humems method to deionized water, ultrasonically dispersing for 1 hour, then adding a 15% by mass nickel acetate aqueous solution, continuing ultrasonication for 2 hours, pouring liquid nitrogen into it until solidification after the ultrasonication to obtain a precursor, then transferring it to a tube furnace, heating it to 900°C at a heating rate of 5-10°C / min, calcining it for 1 hour, then cooling it to room temperature to obtain a crude carrier, then transferring it to a 10% by mass hydrochloric acid aqueous solution and soaking it for 5 hours, then filtering it, washing it three times with deionized water, and vacuum drying it at 85°C for 12 hours to obtain a carrier; Step S2, adding polyether and 1,3,5-trimethylbenzene to a 50% ethanol aqueous solution by volume, then adding Tris buffer with a pH of 8.5, adding a carrier, stirring at a uniform speed and adding dopamine, continuing stirring and reacting for 30 hours, then centrifuging at a speed of 10000 r / min for 5 minutes, collecting the precipitate, and washing it alternately with anhydrous ethanol and acetone three times to obtain a composite carrier; Step S3, add the composite carrier into a three-necked flask, add o-xylene, then add 4-bromodiphenylamine, sodium tert-butoxide and palladium acetate in sequence, purge under argon atmosphere and stir at high speed for 15 minutes, then dropwise add a solution of tri-tert-butylphosphine in o-xylene, purge with argon for 10 minutes, then heat to 160°C, reflux for 12 hours, and obtain a lithium battery positive electrode material.

2. The method for preparing a positive electrode material for a lithium battery according to claim 1, characterized in that: In step S1, the dosage ratio of graphene oxide, nickel acetate and deionized water is controlled to be 150-200 mg: 15-20 mg: 100 mL.

3. The method for preparing a positive electrode material for a lithium battery according to claim 1, characterized in that: In step S2, the weight ratio of polyether, 1,3,5-trimethylbenzene, Tris buffer, carrier and dopamine is controlled to be 200 mg: 200 mg: 20 mg: 100-150 mg: 50-60 mg.

4. The method for preparing a positive electrode material for a lithium battery according to claim 1, characterized in that: In step S3, the dosage ratio of the composite carrier, 4-bromodiphenylamine, sodium tert-butoxide, palladium acetate, o-xylene and tri-tert-butylphosphine is controlled to be 30-50 mg: 10.24-10.28 mg: 21 mg: 0.4-0.5 mg: 50 mL: 0.4 mmol.

5. The method for preparing a positive electrode material for a lithium battery according to claim 1, characterized in that: The tri-tert-butylphosphine o-xylene solution in step S3 is prepared by mixing tri-tert-butylphosphine and o-xylene in a dosage ratio of 0.4 mmol:10 mL.

6. A positive electrode material for a lithium battery, characterized in that: Prepared by the preparation method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method of porous metal doped lithium manganate / graphene lithium battery positive electrode material

    CN105206799A

  • 3D reticulate porous graphene / lithium iron phosphate composite cathode material and preparation method thereof

    CN109244458A

  • Porous carbon-sulfur composite positive electrode material for lithium-sulfur battery, and preparation method thereof

    CN110649251A

  • Lithium ion battery composite positive electrode material, and preparation method and application thereof

    CN113471414A

  • Preparation method of loaded bimetallic ordered mesoporous carbon-coated graphene material for lithium-sulfur battery

    CN114784258A