A solid-state lithium / sodium battery composite cathode material and its preparation method

By preparing composite cathode materials with high or low crystallinity of MAx, solid electrolyte, and electronic conductive agent, the problem of low energy density of lithium-free/sodium composite cathode materials was solved, the voltage and capacity of all-solid-state lithium/sodium batteries were improved, and higher cycle stability was achieved.

CN117012945BActive Publication Date: 2026-11-17HEFEI GUNING JIYUAN NEW ENERGY TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311048292.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-18
Publication Date
2026-11-17
Estimated Expiration
2043-08-18

AI Technical Summary

Technical Problem

Existing lithium/sodium composite cathode materials have low energy density and are easily soluble in lithium-ion battery electrolytes, which limits the performance improvement of all-solid-state batteries.

Method used

All-solid-state lithium/sodium battery composite cathode materials are prepared by ball milling or grinding using highly crystalline or low-crystalline MAx, solid electrolyte, and electronic conductive agent. The preferred MAx components include transition metal ions and anions, combined with specific solid electrolyte and electronic conductive agent. The preparation process is carried out under a protective atmosphere.

Benefits of technology

The voltage and capacity of all-solid-state lithium/sodium batteries have been improved, achieving higher cycle stability and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117012945B_ABST
    Figure CN117012945B_ABST
Patent Text Reader

Abstract

This invention provides an all-solid-state lithium / sodium battery composite cathode material and its preparation method, belonging to the field of all-solid-state battery technology. The all-solid-state lithium / sodium battery composite cathode material of this invention is composed of highly crystalline or low-crystalline MA. x It is prepared by solid electrolyte and electronic conductive agent, among which high crystallinity MA x The crystallinity is 80-100%, and the low crystallinity MA x The crystallinity is 0-30%, MA x In this paper, M represents a transition metal ion, A represents a -1 or -2 valent anion, and 0.5 ≤ x ≤ 6. An all-solid-state lithium / sodium battery was fabricated using the all-solid-state lithium / sodium battery composite cathode material of this invention. Performance tests on the all-solid-state lithium / sodium battery showed that it exhibited high voltage and capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of all-solid-state battery technology, and in particular to an all-solid-state lithium / sodium battery composite cathode material and its preparation method. Background Technology

[0002] Safe, high-energy-density batteries are key to achieving dual-carbon goals. Halogen-rich but lithium / sodium-free solid-state compound cathodes have the potential to provide high specific capacity, and their flexibility and resistance to breakage contribute to high cycle stability. However, such cathode materials are readily soluble in the electrolytes of currently commercial lithium-ion batteries, and therefore have not been extensively studied in the past few decades. For all-solid-state batteries using solid electrolytes, this problem of active material dissolution does not exist. Therefore, with all-solid-state battery technology maturing and moving towards commercialization, developing high-energy-density lithium / sodium-free composite cathode materials is of significant technological importance as it fully leverages the advantages of all-solid-state batteries. Summary of the Invention

[0003] The purpose of this invention is to provide an all-solid-state lithium / sodium battery composite cathode material and its preparation method, so as to solve the problem of low energy density of lithium / sodium composite cathode materials in the prior art.

[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0005] This invention provides an all-solid-state lithium / sodium battery composite cathode material, which is composed of highly crystalline or low-crystalline MA. x It is prepared by solid electrolyte and electronic conductive agent, among which high crystallinity MA x The crystallinity is 80-100%, and the low crystallinity MA x The crystallinity is 0-30%, MA x In this context, M represents a transition metal ion, A represents a -1 valent anion or a -2 valent anion, and 0.5 ≤ x ≤ 6.

[0006] Preferably, the transition metal ion is Ag. + W 6+ 、Nb 5+ Mo 5+ V 3+ V 5+ Cr 3+ Fe 3+ Cu 2+ Ti 3+ Ta 5 + Mn 3+ Mn 5+ Co 2+ and Ni3+ One or more of the following; the -1 valent anion or -2 valent anion is F - Cl - O 2- and S 2- One or more of the following; the solid electrolyte contains Li3Zr 0.75 OCl4, Li 1.75 ZrO 0.5 Cl 4.75 Or Li3InCl6; the electronically conductive agent is one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, carbon black, and graphene.

[0007] Preferably, the highly crystalline or low crystalline MA x The mass ratio of solid electrolyte to electronic conductive agent is 9-y:y:1, where 1≤y≤6.

[0008] Preferably, the low crystallinity MA x The preparation method is as follows: under a protective atmosphere, highly crystalline MA is... x Simply perform ball milling.

[0009] Preferably, the protective atmosphere is an argon atmosphere or a dry air atmosphere.

[0010] Preferably, the ball milling process is performed at a rotation speed of 300–700 rpm, a ball-to-material ratio of 5:1–100:1, and a time of 1–100 h.

[0011] This invention provides a method for preparing an all-solid-state lithium / sodium battery composite cathode material, comprising the following steps: under a protective atmosphere, reacting highly crystalline or low-crystalline MA... x The solid electrolyte and electronic conductive agent can be mixed and then ground or ball-milled.

[0012] Preferably, the grinding time is 0.1 to 10 hours; the ball milling speed is 100 to 250 rpm, the ball-to-material ratio is 5:1 to 100:1, and the time is 1 to 100 hours.

[0013] The beneficial effects of this invention are:

[0014] Compared with existing technologies, this invention provides an all-solid-state lithium / sodium battery composite cathode material, composed of highly crystalline or low-crystalline MA. x It is prepared by solid electrolyte and electronic conductive agent, wherein MA x In this paper, M represents a transition metal ion, A represents a -1 or -2 valent anion, and 0.5 ≤ x ≤ 6. All-solid-state batteries made using the all-solid-state lithium / sodium battery composite cathode material provided by this invention exhibit high voltage and capacity. Attached Figure Description

[0015] Figure 1 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 1 are shown.

[0016] Figure 2 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 2 are shown.

[0017] Figure 3 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 3 are shown.

[0018] Figure 4 The capacity-cycle count diagram is shown for the all-solid-state lithium battery prepared in Example 3.

[0019] Figure 5 The charge-discharge curve of the all-solid-state lithium battery prepared in Example 4 is shown.

[0020] Figure 6 The capacity-cycle count diagram is shown for the all-solid-state lithium battery prepared in Example 4.

[0021] Figure 7 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 5 are shown.

[0022] Figure 8 The capacity-cycle count diagram is shown for the all-solid-state lithium battery prepared in Example 5.

[0023] Figure 9 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 6 are shown.

[0024] Figure 10 The capacity-cycle count diagram is shown for the all-solid-state lithium battery prepared in Example 6.

[0025] Figure 11 The charge-discharge curve of the all-solid-state lithium battery prepared in Example 7;

[0026] Figure 12 The capacity-cycle count diagram is shown for the all-solid-state lithium battery prepared in Example 7.

[0027] Figure 13 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 8 are shown.

[0028] Figure 14 The capacity-cycle count diagram of the all-solid-state lithium battery prepared in Example 8;

[0029] Figure 15 Charge-discharge curves of the all-solid-state lithium battery prepared in Example 9;

[0030] Figure 16 The charge-discharge curves of the all-solid-state lithium battery prepared in Example 10 are shown. Detailed Implementation

[0031] This invention provides an all-solid-state lithium / sodium battery composite cathode material, which is composed of highly crystalline or low-crystalline MA. x It is prepared by solid electrolyte and electronic conductive agent, among which high crystallinity MA x The crystallinity is 80-100%, and the low crystallinity MA x The crystallinity is 0-30%, MA x In this context, M represents a transition metal ion, A represents a -1 valent anion or a -2 valent anion, and 0.5 ≤ x ≤ 6.

[0032] In this invention, high crystallinity MA x The crystallinity is preferably 85-100%, more preferably 90-100%, and low crystallinity MA x The crystallinity is preferably 5-25%, more preferably 10-20%.

[0033] In this invention, the MA x M is a transition metal ion, A is a -1 valent anion or a -2 valent anion, 0.5≤x≤6, and x is preferably 1, 2, 2.5, 3, 5 or 6, and more preferably 2.5, 3, 5 or 6.

[0034] In this invention, the transition metal ion is Ag. + W 6+ 、Nb 5+ Mo 5+ V 3+ V 5+ Cr 3+ Fe 3+ Cu 2+ Ti 3+ Ta 5+ Mn 3+ Mn 5+ Co 2+ and Ni 3+ One or more of them, preferably W 6+ 、Nb 5+ V 3+ V 5+ Mo 5+ Fe 3+ Co 2+ and Ni 3+ One or more of them, more preferably W 6+ 、Nb 5+ V 3+ V 5+ Mo 5+ and Fe 3+One or more of the following; the -1 valent anion or -2 valent anion is F - Cl - O 2- and S 2- One or more of them, preferably F - Cl - and O 2- One or more of them, more preferably F - or Cl - The solid electrolyte contains Li3Zr. 0.75 OCl4, Li 1.75 ZrO 0.5 Cl 4.75 Or Li3InCl6; preferably Li3Zr 0.75 OCl4 or Li 1.75 ZrO 0.5 Cl 4.75 Li3Zr is further preferred. 0.75 OCl4; the electronically conductive agent is one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, carbon black and graphene, preferably one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes and carbon black, and more preferably multi-walled carbon nanotubes and / or single-walled carbon nanotubes.

[0035] In this invention, the highly crystalline or low-crystalline MA x The mass ratio of solid electrolyte to electronic conductive agent is 9-y:y:1, where 1≤y≤6, preferably 2≤y≤5, and more preferably 3, 4 or 5.

[0036] In this invention, the low-crystallinity MA x The preparation method is as follows: under a protective atmosphere, highly crystalline MA is... x Simply perform ball milling.

[0037] In this invention, the protective atmosphere is an argon atmosphere or a dry air atmosphere, preferably an argon atmosphere, and more preferably an argon atmosphere with H2O < 0.01 ppm and O2 < 0.01 ppm.

[0038] In this invention, the ball milling speed is 300-700 rpm, preferably 350-650 rpm, and more preferably 400-600 rpm; the ball-to-material ratio is 5:1-100:1, preferably 10:1-90:1, and more preferably 20:1-80:1; and the time is 1-100 h, preferably 5-95 h, and more preferably 10-90 h.

[0039] This invention provides a method for preparing an all-solid-state lithium / sodium battery composite cathode material, comprising the following steps: under a protective atmosphere, reacting highly crystalline or low-crystalline MA... x The solid electrolyte and electronic conductive agent can be mixed and then ground or ball-milled.

[0040] In this invention, the preparation of the all-solid-state lithium / sodium battery composite cathode material is preferably carried out under an argon atmosphere or a dry air atmosphere, preferably an argon atmosphere, and more preferably an argon atmosphere with H2O < 0.01 ppm and O2 < 0.01 ppm.

[0041] In this invention, the grinding time is 0.1–10 h, preferably 1–9 h, and more preferably 2–8 h; the ball milling speed is 100–250 rpm, preferably 120–220 rpm, and more preferably 150–200 rpm; the ball-to-material ratio is 5:1–100:1, preferably 10:1–90:1, and more preferably 20:1–80:1; and the time is 1–100 h, preferably 5–95 h, and more preferably 10–90 h.

[0042] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0043] Example 1

[0044] FeCl3 and Li3Zr with 100% crystallinity were weighed in a mass ratio of 4:5:1. 0.75 Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 20:1 and ball-milled at 150rpm for 8h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0045] Weigh out 6 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 150MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 150MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 300 MPa to obtain a solid-state lithium / sodium battery composite cathode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite cathode sheet to obtain a solid-state lithium battery.

[0046] The performance of the all-solid-state lithium battery in Example 1 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 41 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 3.7V at room temperature (vs. Li / Li). + ), with a capacity of 137mAh·g -1 .

[0047] Example 2

[0048] Weigh out WCl6 and Li3Zr with a crystallinity of 90% according to a mass ratio of 5:4:1. 0.75 Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 40:1 and ball-milled at 250rpm for 10h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0049] Weigh out 4.62 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 100MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 200MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 500 MPa to obtain a fully solid-state lithium / sodium battery composite positive electrode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the fully solid-state lithium / sodium battery composite positive electrode sheet to obtain a fully solid-state lithium battery.

[0050] The performance of the all-solid-state lithium battery in Example 2 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 216 mA·g. -1 The test results show that the operating voltage of the all-solid-state lithium battery at room temperature is 2.4V (vs. Li / Li). + ), with a capacity of 268mAh·g -1 .

[0051] Example 3

[0052] MoCl5 and Li3Zr with a crystallinity of 80% were weighed in a mass ratio of 5:4:1. 0.75 Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 30:1 and ball-milled at 250rpm for 30h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0053] Weigh out 4.41 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 200MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 100MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 400 MPa to obtain a solid-state lithium / sodium battery composite cathode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite cathode sheet to obtain a solid-state lithium battery.

[0054] The performance of the all-solid-state lithium battery in Example 3 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 226 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 3.4V at room temperature (vs. Li / Li). + ), with a capacity of 145mAh·g -1 And it can still achieve 135.6 mAh·g after 100 cycles. -1 The discharge capacity and capacity retention rate are 83.2%.

[0055] Example 4

[0056] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 20 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity FeCl₃ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 500 rpm for 40 hours to obtain 5% crystallinity FeCl₃. Then, low-crystallinity FeCl₃ and Li₃Zr were weighed in a mass ratio of 5:4:1. 0.75Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 50:1 and ball-milled at 250rpm for 15h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0057] Weigh out 6.71 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 150MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 100MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 350 MPa to obtain a solid-state lithium / sodium battery composite cathode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite cathode sheet to obtain a solid-state lithium battery.

[0058] The performance of the all-solid-state lithium battery in Example 4 was tested. The test was conducted under a pressure of 1.5 tons and a current density of 30 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 1.7V at room temperature (vs. Li / Li). + ), with a capacity of 544mAh·g -1 And it can still achieve 575.8 mAh·g after 100 cycles. -1 The discharge capacity and 96.6% capacity retention

[0059] Example 5

[0060] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 30 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity WCl₆ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 300 rpm for 60 hours to obtain 10% crystallinity WCl₆. Low-crystallinity WCl₆ and Li₃Zr were then weighed in a mass ratio of 5:4:1. 0.75Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 90:1 and ball-milled at 100rpm for 1h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0061] Weigh out 4.8 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 120MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 180MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 450 MPa to obtain a solid-state lithium / sodium battery composite positive electrode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite positive electrode sheet to obtain a solid-state lithium battery.

[0062] The performance of the all-solid-state lithium battery in Example 5 was tested. The test was conducted under a pressure of 1.5 tons and a current density of 80 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 3.1V at room temperature (vs. Li / Li). + ), with a capacity of 165mAh·g -1 And it can still achieve 111.3mAh g after 1000 cycles. -1 The discharge capacity and capacity retention rate are 66.2%.

[0063] Example 6

[0064] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 90 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity MoCl₅ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 600 rpm for 20 hours to obtain 20% crystallinity MoCl₅. Low-crystallinity MoCl₅ and Li₃Zr were then weighed in a mass ratio of 5:4:1. 0.75Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 60:1 and ball-milled at 120rpm for 80h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0065] Weigh out 4.47 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 150MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 150MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 450 MPa to obtain a solid-state lithium / sodium battery composite positive electrode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite positive electrode sheet to obtain a solid-state lithium battery.

[0066] The performance of the all-solid-state lithium battery in Example 6 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 87 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 3.3V at room temperature (vs. Li / Li). + ), with a capacity of 152mAh·g -1 And it can still achieve 131mAh g after 950 cycles. -1 The discharge capacity and 80% capacity retention rate.

[0067] Example 7

[0068] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 50 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity NbCl₅ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 450 rpm for 50 hours to obtain NbCl₅ with 30% crystallinity. Then, low-crystallinity NbCl₅ and Li₃Zr were weighed according to a mass ratio of 6:3:1. 0.75Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 50:1 and ball-milled at 130 pm for 60 hours to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0069] Weigh out 5.04 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 160MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 140 MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 480 MPa to obtain a solid-state lithium / sodium battery composite cathode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite cathode sheet to obtain a solid-state lithium battery.

[0070] The performance of the all-solid-state lithium battery in Example 7 was tested under a pressure of 1.5 tons and a current density of 77 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 2.8V at room temperature (vs. Li / Li). + ), with a capacity of 151mAh·g -1 And it can still achieve 124mAh g after 800 cycles. -1 The capacity and 81% capacity retention rate.

[0071] Example 8

[0072] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 50 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity VCl₃ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 600 rpm for 25 hours to obtain 0% crystallinity VCl₃. Low-crystallinity VCl₃ and Li₃Zr were then weighed in a mass ratio of 3:6:1. 0.75Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 70:1 and ball-milled at 100pm for 90h to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0073] Weigh out 4.7 mg of all-solid-state lithium / sodium battery composite cathode material and 20 mg of Li3Zr. 0.75 OCl4 and 50mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 180MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 120MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 420 MPa to obtain a fully solid-state lithium / sodium battery composite positive electrode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the fully solid-state lithium / sodium battery composite positive electrode sheet to obtain a fully solid-state lithium battery.

[0074] The performance of the all-solid-state lithium battery in Example 8 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 83 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 2.7V at room temperature (vs. Li / Li). + ), with a capacity of 145mAh·g -1 And it can still achieve 106.2mAh g after 1000 cycles. -1 The discharge capacity and capacity retention rate are 64.7%.

[0075] Example 9

[0076] Weigh out V₂O₅ and Li₃Zr with 100% crystallinity in a mass ratio of 5:4:1. 0.75 Three powders, namely OCl4 and multi-walled carbon nanotubes, were weighed in total (1 g). The powders were ground in an agate mortar for 30 min under an argon atmosphere (H2O < 0.01 ppm, O2 < 0.01 ppm) to obtain a solid-state lithium / sodium battery composite cathode material.

[0077] Weigh out 5.72 mg of all-solid-state lithium / sodium battery composite cathode material and 30 mg of Li3Zr. 0.75OCl4 and 60mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 200MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75 OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 100MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a sheet under a pressure of 300 MPa to obtain a solid-state lithium / sodium battery composite cathode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the solid-state lithium / sodium battery composite cathode sheet to obtain a solid-state lithium battery.

[0078] The performance of the all-solid-state lithium battery in Example 9 was tested. The test was conducted under a pressure of 1.5 tons, with a current density of 137 mA·g. -1 The test results show that the all-solid-state lithium battery operates at 1.8V at room temperature (vs. Li / Li). + ), with a capacity of 120mAh·g -1 .

[0079] Example 10

[0080] In an argon atmosphere glove box (H₂O < 0.01 ppm, O₂ < 0.01 ppm), 50 g of zirconia balls (5 mm in diameter) and 1 g of 100% crystallinity FeF₃ were weighed and poured into an 80 mL zirconia ball mill jar. The mixture was ball-milled at 300 rpm for 70 hours to obtain FeF₃ with 25% crystallinity. Then, low-crystallinity FeF₃ and Li₃Zr were weighed in a mass ratio of 5:4:1. 0.75 Three powders, OCl4 and multi-walled carbon nanotubes, were weighed, with a total mass of 1g. Under an argon atmosphere with H2O < 0.01ppm and O2 < 0.01ppm, the weighed powder was placed in a high-energy ball mill with a ball-to-powder ratio of 50:1 and ball-milled at 200 pm for 15 hours to obtain an all-solid-state lithium / sodium battery composite cathode material.

[0081] Weigh out 7.58 mg of all-solid-state lithium / sodium battery composite cathode material and 25 mg of Li3Zr. 0.75 OCl4 and 55mg Li6PS5Cl powder were first poured into a polyetheretherketone mold (10mm in diameter) and pressed into sheets under a pressure of 170MPa to obtain Li6PS5Cl sheets; then Li3Zr was added. 0.75OCl4 powder was uniformly spread on Li6PS5Cl sheets and pressed into sheets under a pressure of 130 MPa; then, the all-solid-state lithium / sodium battery composite cathode material was uniformly spread on Li3Zr. 0.75 On the OCl4 sheet, a sheet is pressed into a film under a pressure of 440 MPa to obtain a fully solid-state lithium / sodium battery composite positive electrode sheet; finally, an indium sheet (100 μm) and a lithium sheet (50 μm) are sequentially pasted on the side away from the fully solid-state lithium / sodium battery composite positive electrode sheet to obtain a fully solid-state lithium battery.

[0082] The performance of the all-solid-state lithium battery in Example 10 was tested under a pressure of 1.5 tons and a current density of 51 mA·g. -1 The test results showed that the battery's operating voltage at room temperature was 2.8V (vs. Li / Li). + ), with a capacity of 79mAh·g -1 .

[0083] As can be seen from the above embodiments, the present invention provides an all-solid-state lithium / sodium battery composite cathode material and its preparation method. The all-solid-state lithium / sodium battery composite cathode material of the present invention is composed of highly crystalline or low-crystalline MA. x It is prepared by solid electrolyte and electronic conductive agent, among which high crystallinity MA x The crystallinity is 80-100%, and the low crystallinity MA x The crystallinity is 0-30%, MA x In this paper, M represents a transition metal ion, A represents a -1 or -2 valent anion, and 0.5 ≤ x ≤ 6. An all-solid-state lithium / sodium battery was fabricated using the all-solid-state lithium / sodium battery composite cathode material of this invention. Performance tests on the all-solid-state lithium / sodium battery showed that it exhibited high voltage and capacity.

[0084] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A composite cathode material for all-solid-state lithium / sodium batteries, characterized in that, All-solid-state lithium / sodium battery composite cathode materials are made of highly crystalline or low-crystalline MA x It is prepared by solid electrolyte and electronic conductive agent, among which high crystallinity MA x The crystallinity is 80-100%, and the low crystallinity MA x The crystallinity is 0~30%, MA x In this context, M represents a transition metal ion, and A represents Cl-. - 0.5≤ x ≤6; the transition metal ion is Ag + , W 6+ , Nb 5+ , Mo 5+ , V 3+ , V 5+ , Cr 3+ , Fe 3+ , Cu 2+ , Ta 5+ , Mn 3+ , Mn 5+ , Co 2+ , and Ni 3+ . The solid-state electrolyte is Li3Zr 0.75 OC1 4 or Li 1.75 ZrO 0.5 Cl 4.75 ; the high crystallinity or low crystallinity MA x a mass ratio of the solid-state electrolyte and the electron conductive agent is 9-y:y:1, where 1≤y≤6; The preparation method of the all-solid-state lithium / sodium battery composite cathode material includes the following steps: under a protective atmosphere, high-crystallinity or low-crystallinity MA is... x The solid electrolyte and electronic conductive agent can be mixed and then ground or ball-milled. The grinding time is 0.1~10h; the ball milling speed is 100~250rpm, the ball-to-material ratio is 5:1~100:1, and the time is 1~100h.

2. The all-solid-state lithium / sodium battery composite cathode material according to claim 1, characterized in that, The electronically conductive agent comprises one or more of multi-walled carbon nanotubes, single-walled carbon nanotubes, carbon black, and graphene.

3. The all-solid-state lithium / sodium battery composite cathode material according to claim 2, characterized in that, The low crystallinity MA x The preparation method is as follows: under a protective atmosphere, highly crystalline MA is... x Simply perform ball milling.

4. The all-solid-state lithium / sodium battery composite cathode material according to claim 3, characterized in that, The protective atmosphere is an argon atmosphere or a dry air atmosphere.

5. The all-solid-state lithium / sodium battery composite cathode material according to claim 3 or 4, characterized in that, The ball milling process is performed at a speed of 300-700 rpm, a ball-to-material ratio of 5:1-100:1, and a time of 1-100 h.

Citation Information

Patent Citations

  • Composite positive electrode of lithium ion battery as well as preparation method and application to all-solid-state battery thereof

    CN103956458A